Powder core wire and method of making intergranular corrosion resistant austenitic stainless steel structural component
By using powder-core wire and 3D printing technology, elements such as Ti and Nb are added to form carbides, and rare earth oxides are used to optimize the molten pool. This solves the shortcomings of traditional austenitic stainless steel in terms of resistance to intergranular corrosion, and produces efficient and economical intergranular corrosion resistant austenitic stainless steel structural parts, which are suitable for marine engineering, petrochemical and energy fields.
Patent Information
- Application Number
- CN202410678680.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-29
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-05-29
AI Technical Summary
Traditional austenitic stainless steel has shortcomings in resistance to intergranular corrosion, especially in acidic corrosive environments and marine atmospheric service, which easily leads to premature failure of structural components. The composition of existing solid wire materials is difficult to adjust and the cost is high.
Using powder-core wire containing a specific ratio of metal powder and 316 austenitic stainless steel strip, 3D printing technology is used to prepare austenitic stainless steel structural parts resistant to intergranular corrosion. Elements such as Ti and Nb are added to form carbides, and rare earth oxides optimize the molten pool, refine the grains, and improve corrosion resistance.
It has achieved efficient and economical preparation of austenitic stainless steel structural components resistant to intergranular corrosion. These components have excellent resistance to intergranular corrosion and high strength, making them suitable for the manufacture of complex structural components and applicable to marine engineering, petrochemical and energy fields.
Smart Images

Figure CN118371725B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of additive manufacturing 3D printing materials technology, specifically relating to powder core filaments, and also to a method for preparing austenitic stainless steel structural parts resistant to intergranular corrosion. Background Technology
[0002] Austenitic stainless steel is widely used in engineering construction due to its excellent strength, ductility, and corrosion resistance, as well as its relatively low cost. However, with the continuous expansion of its application fields, excellent resistance to intergranular corrosion is required in environments requiring resistance to acidic corrosion and marine atmospheric conditions. Traditional austenitic stainless steels, such as 304 and 316, are prone to intergranular corrosion due to the precipitation of carbides, leading to premature failure of structural components. As one of my country's three pillar materials, the rapid development of modern industry has placed higher demands on the comprehensive mechanical properties of austenitic stainless steel.
[0003] Intergranular corrosion in austenitic stainless steel can usually be addressed by reducing the carbon content and adding strong carbide-forming elements. However, adjusting the composition of solid wire is difficult and costly. In contrast, powder-core wire allows for easier adjustment of its alloy composition and a more precise range of chemical components, making it suitable for new material research and development. It offers greater flexibility, higher cladding efficiency (one-third higher than solid wire), effectively saves energy, and produces denser, higher-performance parts. Therefore, it is considered more suitable for manufacturing austenitic stainless steel structural components.
[0004] Compared to traditional rolling and forging processes for manufacturing austenitic stainless steel structural parts, arc additive manufacturing 3D printing technology based on wire is more efficient, flexible, and economical. It can form complex structural parts. When using self-developed austenitic stainless steel powder core wire for additive manufacturing to 3D print austenitic stainless steel structural parts, it has stable welding processability, high cladding efficiency, short manufacturing cycle of formed structural parts, beautiful appearance without collapse, and excellent resistance to intergranular corrosion, making up for the lack of raw materials for 3D printing. Summary of the Invention
[0005] The first objective of this invention is to provide a powder-core filament material that can be used for 3D printing austenitic stainless steel structural parts, which has high cladding efficiency and improves the intergranular corrosion resistance of austenitic stainless steel.
[0006] The second objective of this invention is to provide a method for preparing austenitic stainless steel structural components resistant to intergranular corrosion based on powder-core wire as raw material.
[0007] The first technical solution adopted in this invention is: a powder-core wire material, comprising metal powder and steel strip. The metal powder composition consists of the following components by mass percentage: graphene 0.07%–0.08%, chromium powder 20.0%–24.0%, nickel powder 15.6%–16.0%, molybdenum powder 4.3%–4.5%, silicon powder 1.2%–2.2%, manganese powder 2.5%–3.5%, titanium powder 1.0%–2.0%, niobium powder 2.0%–3.0%, tantalum powder 0.05%–0.15%, yttrium oxide 0.5%–1.5%, cerium oxide 0.2%–0.6%, with the remainder being iron powder. The sum of the mass percentages of the above components is 100%. The steel strip is 316 austenitic stainless steel strip, and the metal powder filling rate is 22%–30%.
[0008] The second technical solution adopted in this invention is: a method for preparing austenitic stainless steel structural components resistant to intergranular corrosion, which uses 3D printing technology to clad powder-core wire onto the surface of a 316 steel plate, thereby obtaining austenitic stainless steel structural components resistant to intergranular corrosion; specifically, it is carried out according to the following steps:
[0009] Step 1: Weigh out the following components by mass percentage: 0.07%–0.08% graphene, 20.0%–24.0% chromium powder, 15.6%–16.0% nickel powder, 4.3%–4.5% molybdenum powder, 1.2%–2.2% silicon powder, 2.5%–3.5% manganese powder, 1.0%–2.0% titanium powder, 2.0%–3.0% niobium powder, 0.05%–0.15% tantalum powder, 0.5%–1.5% yttrium oxide, 0.2%–0.6% cerium oxide, with the remainder being iron powder. Mix the weighed alloy powders using a V-type powder mixer to ensure thorough and uniform mixing. Then place the mixture in a tube furnace and heat and maintain the temperature in a pure argon atmosphere.
[0010] Step 2: Wipe the 316 austenitic stainless steel strip with acetone to remove oil stains and dirt from the surface, then put it into an electric resistance furnace and keep it at a temperature of 100-150℃ for 1-1.5 hours to ensure that the surface of the steel strip is smooth.
[0011] Step 3: Add the alloy powder obtained in Step 1 into the U-shaped groove of the steel strip obtained in Step 2, and make a 2.30mm welding wire by closing the forming roll of the fully automatic wire drawing machine. Finally, make a 1.20mm powder core wire by gradually reducing the diameter.
[0012] Step 4: Assemble the prepared powder core wire from Step 3 into the fully automatic welding robot. After determining the welding process, plan the welding path and layer height and input them into the welding robot. Select 316 steel plate as the workpiece substrate. Use an angle grinder to remove the oxide scale and impurities on the surface of the steel plate and grind the surface smooth. Then run the welding machine command and use MIG welding as the heat source to 3D print austenitic stainless steel structural parts.
[0013] The second technical solution of this invention is also characterized by the following:
[0014] In step 1, the powder mixer speed is 70 r / min and the mixing time is 3 h; the heat preservation temperature in step 1 is 200-300℃ and the heat preservation time is 2-2.5 h to remove moisture from the alloy powder.
[0015] In step 2, the steel strip has a width of 0.7 mm and a thickness of 0.2 mm.
[0016] In step 4, the austenitic stainless steel structural parts are modeled using 3DS MAX modeling software, and slicing is performed using CAM software.
[0017] In step 4, the 3D printing process parameters are as follows: cladding voltage is 20.0V, cladding current is 180.0A, welding speed is 0.25m / min; welding swing is 0.8mm, welding torch is raised 4mm per layer, shielding gas is 99.99% argon, and gas flow rate is 10-15L / min.
[0018] The beneficial effects of this invention are:
[0019] (1) This invention provides a powder core wire for additive manufacturing of austenitic stainless steel resistant to intergranular corrosion. Compared with solid wire, its composition is easy to adjust, the preparation cycle is short, and continuous production can be achieved, thereby greatly saving manufacturing costs. It can be used in the forming and manufacturing of complex austenitic stainless steel in high-end fields such as marine engineering, petrochemicals and energy that are resistant to intergranular corrosion.
[0020] (2) The present invention adds Ti, Nb and Ta elements to the wire material to form carbides, which can avoid the "chromium depletion" phenomenon in austenitic stainless steel and improve the resistance of austenitic stainless steel to intergranular corrosion.
[0021] (3) The powder core wire of the present invention optimizes the component ratio by adding rare earth oxides to adjust the melting point, viscosity and surface tension of the molten pool, so that a dense slag shell is formed on the surface of the molten pool during the solidification process, ensuring a smooth weld bead. The addition of rare earth oxides can refine the grains. The grain refinement reduces the degree of element segregation during the cladding process, and the microstructure composition is more uniform, which improves the resistance of the structural parts to intergranular corrosion.
[0022] (4) The powder core wire for additive manufacturing of austenitic stainless steel with resistance to intergranular corrosion of the present invention fills the market gap. When 3D printing austenitic stainless steel structural parts, there is little spatter, the electric arc is stable, no pore inclusions are generated, the structural parts are beautifully formed, and it has both excellent resistance to intergranular corrosion and high strength. Moreover, according to actual needs, austenitic stainless steel structural parts with different shapes can be printed using self-developed wire as raw material. Attached Figure Description
[0023] Figure 1 This is a stress-strain curve of the austenitic stainless steel structural component prepared in Example 1 of the present invention;
[0024] Figure 2 This is a stress-strain curve of the austenitic stainless steel structural component prepared in Example 2 of the present invention;
[0025] Figure 3 This is a stress-strain curve of the austenitic stainless steel structural component prepared in Example 3 of the present invention;
[0026] Figure 4 This is a stress-strain curve of the austenitic stainless steel structural component prepared in Example 4 of the present invention;
[0027] Figure 5 This is a stress-strain curve of the austenitic stainless steel structural component prepared in Example 5 of the present invention. Detailed Implementation
[0028] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments.
[0029] The powder-core filament of the present invention comprises a core and an outer sheath. The core is composed of the following components by mass percentage: 0.07%–0.08% graphene, 20.0%–24.0% chromium powder, 15.6%–16.0% nickel powder, 4.3%–4.5% molybdenum powder, 1.2%–2.2% silicon powder, 2.5%–3.5% manganese powder, 1.0%–2.0% titanium powder, 2.0%–3.0% niobium powder, 0.05%–0.15% tantalum powder, 0.5%–1.5% yttrium oxide, 0.2%–0.6% cerium oxide, and the remainder being iron powder. The outer sheath is made of 316 austenitic stainless steel strip, and the core filling rate is 22%–30%.
[0030] The roles and functions of each component in this powder-core filament are as follows:
[0031] Ni can effectively improve the strength of stainless steel, with little effect on plasticity. In addition, as an austenite forming element, adding Ni promotes the progressive transformation of ferrite to austenite and stabilizes the original austenite, thus controlling the austenite content in stainless steel.
[0032] Mo, as a major constituent element in stainless steel, can improve corrosion resistance in reducing media, especially the resistance to pitting corrosion and stress corrosion. However, the amount of Mo added to austenitic stainless steel should not be too much, as Mo is a ferritinizing element and excessive addition will promote the formation of precipitates within the ferrite phase.
[0033] Si and Mn elements can play a solid solution strengthening role in austenite and ferrite, thereby improving the strength and hardness of stainless steel. At the same time, Si and Mn can play a joint deoxidation role, which can ensure the quality of weld.
[0034] As the most abundant alloying element, Cr can improve the strength and hardness of stainless steel. It also forms a stable and dense passivation film on the surface of stainless steel, preventing corrosive media from penetrating the interior of the steel and thus enhancing the overall corrosion resistance of the steel. However, in dilute H2SO4, H3PO4, and organic acid corrosive environments, carbon readily forms Cr. 23 C6 makes structural components susceptible to intergranular corrosion.
[0035] Because Cr readily combines with C to form Cr 23 C6 leads to localized "chromium depletion," making it susceptible to intergranular corrosion. Therefore, the addition of strong carbide-forming elements such as Ti and Nb preferentially combines with C to form carbides in austenitic stainless steel, thereby improving resistance to intergranular corrosion, enhancing the steel's plasticity and impact toughness. The addition of Nb can play a solid solution strengthening role, refining the grains and thus improving the strength and plasticity of stainless steel.
[0036] The addition of Ta can form a stable and dense Ta2O5 protective film on the surface of structural components, thereby improving impact toughness and providing extremely high corrosion resistance. Secondly, Ta can also combine with C to form carbides, which improves resistance to intergranular corrosion.
[0037] The addition of rare earth oxides Y2O3 and CeO2 can change the viscosity of the slag, improve the slag removal ability, and purify the weld bead; secondly, it stabilizes the formation of the oxide film, thereby improving the structural components' resistance to intergranular corrosion. CeO2 can also act as a heterogeneous nucleation agent, refining the grains and improving the strength and hardness of the structural components.
[0038] As a two-dimensional reinforcing material, graphene has the advantage of isotropy in the horizontal direction, which makes the structural components have the same performance in all directions. In addition, the addition of graphene can significantly refine the grain size and improve hardness and strength.
[0039] The present invention will now be described in detail with reference to the accompanying drawings and specific embodiments.
[0040] Example 1
[0041] The method for preparing the intergranular corrosion resistant austenitic stainless steel structural component of the present invention comprises the following specific steps:
[0042] Weigh out the following metal powders by mass percentage: 0.08% graphene, 20.0% chromium powder, 15.6% nickel powder, 4.3% molybdenum powder, 1.2% silicon powder, 2.2% manganese powder, 1.0% titanium powder, 2.0% niobium powder, 0.05% tantalum powder, 0.5% yttrium oxide, 0.2% cerium oxide, with the remainder being iron powder. The sum of the mass percentages of the above components is 100%. Mix the weighed alloy powders using a V-type powder mixer at a speed of 70 r / min for 3 hours to ensure thorough and uniform mixing. Then place the mixture in a tube furnace and heat and hold it in a pure argon atmosphere at a temperature of 200-300℃ for 2-2.5 hours to remove moisture from the alloy powder.
[0043] Step 2: Wipe the 316 austenitic stainless steel strip with acetone to remove surface oil and dirt, then place it in an electric resistance furnace and hold it at 100-150℃ for 1-1.5 hours. Ensure the steel strip surface is smooth.
[0044] Step 3: Place the clean austenitic stainless steel strip with a width of 7mm and a thickness of 0.2mm from Step 2 onto the wire drawing machine, and then roll it into a U-shaped groove through a groove pressing process. Add the alloy powder obtained in Step 1 into the U-shaped groove, and after passing through the closed forming roller of the fully automatic wire drawing machine, it is made into a 2.30mm welding wire. Finally, it is made into a 1.20mm powder core wire by gradually reducing the diameter.
[0045] Step 4: Model the austenitic stainless steel structural component using 3DS MAX modeling software. Use CAM software for slicing. Select a 316 stainless steel plate with dimensions of 300mm × 200mm × 15mm as the workpiece substrate. Use an angle grinder to remove surface oxide scale and impurities, smoothing the surface. Assemble the powder-core wire into a fully automated welding robot. Under pre-set models and parameters, perform layer-by-layer cladding of the part, gradually adding material from line to surface to volume to obtain the structural component. Use MIG welding as the heat source for 3D printing to obtain the austenitic stainless steel structural component of this invention. Process parameters are: cladding voltage 20.0V, cladding current 180.0A, welding speed 0.25m / min; welding swing amplitude 0.8mm, welding torch height 4mm per layer, shielding gas 99.99% argon, gas flow rate 10-15L / min.
[0046] The stress-strain test curve results of the structural component in Embodiment 1 of the present invention are as follows: Figure 1 As shown, the tensile strength of the austenitic stainless steel structural component is 554 MPa. To evaluate the degree of intergranular corrosion sensitization of the structural component, the sensitization coefficient (DOS) was calculated using cyclic polarization curves to assess the intergranular corrosion resistance of the austenitic stainless steel structural component. The test solution was 1 mol / L H2SO4 + 0.01 mol / L KSCN, and the sensitization coefficient of the structural component in Example 1 was measured to be 1.1%.
[0047] Example 2
[0048] The method for preparing the intergranular corrosion resistant austenitic stainless steel structural component of the present invention comprises the following specific steps:
[0049] Step 1: Weigh the following metal powders by mass percentage: graphene 0.07%, chromium powder 21.0%, nickel powder 15.8%, molybdenum powder 4.4%, silicon powder 2.0%, manganese powder 2.4%, titanium powder 1.0%, niobium powder 3.0%, tantalum powder 0.15%, yttrium oxide 1.0%, cerium oxide 0.6%, with the remainder being iron powder. The sum of the mass percentages of the above components is 100%. Mix the weighed alloy powders using a V-type powder mixer at a speed of 70 r / min for 3 hours to ensure thorough and uniform mixing. Then place the mixture in a tube furnace and heat and hold it in a pure argon atmosphere at a temperature of 200-300℃ for 2-2.5 hours to remove moisture from the alloy powder.
[0050] Step 2: Wipe the 316 austenitic stainless steel strip with acetone to remove surface oil and dirt, then place it in an electric resistance furnace and hold it at 100-150℃ for 1-1.5 hours. Ensure the steel strip surface is smooth.
[0051] Step 3: Place the clean austenitic stainless steel strip with a width of 7mm and a thickness of 0.2mm from Step 2 onto the wire drawing machine, and then roll it into a U-shaped groove through a groove pressing process. Add the alloy powder obtained in Step 1 into the U-shaped groove, and after passing through the closed forming roller of the fully automatic wire drawing machine, it is made into a 2.30mm welding wire. Finally, it is made into a 1.20mm powder core wire by gradually reducing the diameter.
[0052] Step 4: Model the austenitic stainless steel structural component using 3DS MAX modeling software. Use CAM software for slicing. Select a 316 stainless steel plate with dimensions of 300mm × 200mm × 15mm as the workpiece substrate. Use an angle grinder to remove surface oxide scale and impurities, smoothing the surface. Assemble the powder-core wire into a fully automated welding robot. Under pre-set models and parameters, perform layer-by-layer cladding of the part, gradually adding material from line to surface to volume to obtain the structural component. Use MIG welding as the heat source for 3D printing to obtain the austenitic stainless steel structural component of this invention. Process parameters are: cladding voltage 20.5V, cladding current 185.0A, welding speed 0.25m / min; welding swing amplitude 0.8mm, welding torch height 4mm per layer, shielding gas 99.99% argon, gas flow rate 10-15L / min.
[0053] The stress-strain test curve results of the structural component in Embodiment 2 of the present invention are as follows: Figure 2As shown, the tensile strength of the austenitic stainless steel structural component is 588 MPa. To evaluate the degree of intergranular corrosion sensitization of the structural component, the sensitization coefficient (DOS) was calculated using cyclic polarization curves to assess the intergranular corrosion resistance of the austenitic stainless steel structural component. The test solution was 1 mol / L H2SO4 + 0.01 mol / L KSCN, and the sensitization coefficient of the structural component in Example 1 was measured to be 0.8%.
[0054] Example 3
[0055] The method for preparing the intergranular corrosion resistant austenitic stainless steel structural component of the present invention comprises the following specific steps:
[0056] Step 1: Weigh the following metal powders by mass percentage: graphene 0.07%, chromium powder 22.0%, nickel powder 16.0%, molybdenum powder 4.5%, silicon powder 1.8%, manganese powder 2.8%, titanium powder 2.0%, niobium powder 2.0%, tantalum powder 0.1%, yttrium oxide 1.5%, cerium oxide 0.4%, with the remainder being iron powder. The sum of the mass percentages of the above components is 100%. Mix the weighed alloy powders using a V-type powder mixer at a speed of 70 r / min for 3 hours to ensure thorough and uniform mixing. Then place the mixture in a tube furnace and heat and hold it in a pure argon atmosphere at a temperature of 200-300℃ for 2-2.5 hours to remove moisture from the alloy powder.
[0057] Step 2: Wipe the 316 austenitic stainless steel strip with acetone to remove surface oil and dirt, then place it in an electric resistance furnace and hold it at 100-150℃ for 1-1.5 hours. Ensure the steel strip surface is smooth.
[0058] Step 3: Place the clean austenitic stainless steel strip with a width of 7mm and a thickness of 0.2mm from Step 2 onto the wire drawing machine, and then roll it into a U-shaped groove through a groove pressing process. Add the alloy powder obtained in Step 1 into the U-shaped groove, and after passing through the closed forming roller of the fully automatic wire drawing machine, it is made into a 2.30mm welding wire. Finally, it is made into a 1.20mm powder core wire by gradually reducing the diameter.
[0059] Step 4: Model the austenitic stainless steel structural component using 3DS MAX modeling software. Use CAM software for slicing. Select a 316 stainless steel plate with dimensions of 300mm × 200mm × 15mm as the workpiece substrate. Use an angle grinder to remove surface oxide scale and impurities, smoothing the surface. Assemble the powder-core wire into a fully automated welding robot. Under pre-set models and parameters, perform layer-by-layer cladding of the part, gradually adding material from line to surface to volume to obtain the structural component. Use MIG welding as the heat source for 3D printing to obtain the austenitic stainless steel structural component of this invention. Process parameters are: cladding voltage 21.0V, cladding current 190.0A, welding speed 0.25m / min; welding swing amplitude 0.8mm, welding torch height 4mm per layer, shielding gas 99.99% argon, gas flow rate 10-15L / min.
[0060] The stress-strain test curve results of the structural component in Embodiment 3 of the present invention are as follows: Figure 3 As shown, the tensile strength of the austenitic stainless steel structural component is 576 MPa. To evaluate the degree of intergranular corrosion sensitization of the structural component, the sensitization coefficient (DOS) was calculated using cyclic polarization curves to assess the intergranular corrosion resistance of the austenitic stainless steel structural component. The test solution was 1 mol / L H2SO4 + 0.01 mol / L KSCN, and the sensitization coefficient of the structural component in Example 1 was measured to be 0.6%.
[0061] Example 4
[0062] The method for preparing the intergranular corrosion resistant austenitic stainless steel structural component of the present invention comprises the following specific steps:
[0063] Step 1: Weigh the following metal powders by mass percentage: graphene 0.08%, chromium powder 23.0%, nickel powder 15.8%, molybdenum powder 4.5%, silicon powder 2.2%, manganese powder 3.2%, titanium powder 2.0%, niobium powder 3.0%, tantalum powder 0.05%, yttrium oxide 0.5%, cerium oxide 0.2%, with the remainder being iron powder. The sum of the mass percentages of the above components is 100%. Mix the weighed alloy powders using a V-type powder mixer at a speed of 70 r / min for 3 hours to ensure thorough and uniform mixing. Then place the mixture in a tube furnace and heat and hold it in a pure argon atmosphere at a temperature of 200-300℃ for 2-2.5 hours to remove moisture from the alloy powder.
[0064] Step 2: Wipe the 316 austenitic stainless steel strip with acetone to remove surface oil and dirt, then place it in an electric resistance furnace and hold it at 100-150℃ for 1-1.5 hours. Ensure the steel strip surface is smooth.
[0065] Step 3: Place the clean austenitic stainless steel strip with a width of 7mm and a thickness of 0.2mm from Step 2 onto the wire drawing machine, and then roll it into a U-shaped groove through a groove pressing process. Add the alloy powder obtained in Step 1 into the U-shaped groove, and after passing through the closed forming roller of the fully automatic wire drawing machine, it is made into a 2.30mm welding wire. Finally, it is made into a 1.20mm powder core wire by gradually reducing the diameter.
[0066] Step 4: Model the austenitic stainless steel structural component using 3DS MAX modeling software. Use CAM software for slicing. Select a 316 stainless steel plate with dimensions of 300mm × 200mm × 15mm as the workpiece substrate. Use an angle grinder to remove surface oxide scale and impurities, smoothing the surface. Assemble the powder-core wire into a fully automated welding robot. Under pre-set models and parameters, perform layer-by-layer cladding of the part, gradually adding material from line to surface to volume to obtain the structural component. Use MIG welding as the heat source for 3D printing to obtain the austenitic stainless steel structural component of this invention. Process parameters are: cladding voltage 21.5V, cladding current 195.0A, welding speed 0.25m / min; welding swing amplitude 0.8mm, welding torch height 4mm per layer, shielding gas 99.99% argon, gas flow rate 10-15L / min.
[0067] The stress-strain test curve results of the structural component in Embodiment 4 of the present invention are as follows: Figure 4 As shown, the tensile strength of the austenitic stainless steel structural component is 594 MPa. To evaluate the degree of intergranular corrosion sensitization of the structural component, the sensitization coefficient (DOS) was calculated using cyclic polarization curves to assess the intergranular corrosion resistance of the austenitic stainless steel structural component. The test solution was 1 mol / L H2SO4 + 0.01 mol / L KSCN, and the sensitization coefficient of the structural component in Example 1 was measured to be 0.5%.
[0068] Example 5
[0069] The method for preparing the intergranular corrosion resistant austenitic stainless steel structural component of the present invention comprises the following specific steps:
[0070] Weigh out the following metal powders by mass percentage: 0.08% graphene, 24.0% chromium powder, 16.0% nickel powder, 4.4% molybdenum powder, 1.6% silicon powder, 3.0% manganese powder, 0.05% tantalum powder, 0.5% yttrium oxide, 0.2% cerium oxide, with the remainder being iron powder. The sum of the mass percentages of the above components is 100%. Mix the weighed alloy powders using a V-type powder mixer at a speed of 70 r / min for 3 hours to ensure thorough and uniform mixing. Then place the mixture in a tube furnace and heat and hold it in a pure argon atmosphere at a temperature of 200-300℃ for 2-2.5 hours to remove moisture from the alloy powders.
[0071] Step 2: Wipe the 316 austenitic stainless steel strip with acetone to remove surface oil and dirt, then place it in an electric resistance furnace and hold it at 100-150℃ for 1-1.5 hours. Ensure the steel strip surface is smooth.
[0072] Step 3: Place the clean austenitic stainless steel strip with a width of 7mm and a thickness of 0.2mm from Step 2 onto the wire drawing machine, and then roll it into a U-shaped groove through a groove pressing process. Add the alloy powder obtained in Step 1 into the U-shaped groove, and after passing through the closed forming roller of the fully automatic wire drawing machine, it is made into a 2.30mm welding wire. Finally, it is made into a 1.20mm powder core wire by gradually reducing the diameter.
[0073] Step 4: Model the austenitic stainless steel structural component using 3DS MAX modeling software. Use CAM software for slicing. Select a 316 stainless steel plate with dimensions of 300mm × 200mm × 15mm as the workpiece substrate. Use an angle grinder to remove surface oxide scale and impurities, smoothing the surface. Assemble the powder-core wire into a fully automated welding robot. Under pre-set models and parameters, perform layer-by-layer cladding of the part, gradually adding material from line to surface to volume to obtain the structural component. Use MIG welding as the heat source for 3D printing to obtain the austenitic stainless steel structural component of this invention. Process parameters are: cladding voltage 22.0V, cladding current 200.0A, welding speed 0.25m / min; welding swing amplitude 0.8mm, welding torch height 4mm per layer, shielding gas 99.99% argon, gas flow rate 10-15L / min.
[0074] The stress-strain test curve results of the structural component in Embodiment 5 of the present invention are as follows: Figure 5 As shown, the tensile strength of the austenitic stainless steel structural component is 625 MPa. To evaluate the degree of intergranular corrosion sensitization of the structural component, the sensitization coefficient (DOS) was calculated using cyclic polarization curves to assess the intergranular corrosion resistance of the austenitic stainless steel structural component. The test solution was 1 mol / L H2SO4 + 0.01 mol / L KSCN. The sensitization coefficient of the structural component in Example 1 was measured to be 0%, indicating that it has good intergranular corrosion resistance.
[0075] Therefore, it can be seen that the stainless steel structural parts prepared by the method of the present invention not only have excellent mechanical properties, but also have good resistance to intergranular corrosion.
Claims
1. A powder-core filament, characterized in that, The core wire comprises a core and an outer sheath. The core is composed of the following components by mass percentage: graphene 0.07%~0.08%, chromium powder 20.0%~24.0%, nickel powder 15.6%~16.0%, molybdenum powder 4.3%~4.5%, silicon powder 1.2%~2.2%, manganese powder 2.5%~3.5%, titanium powder 1.0%~2.0%, niobium powder 2.0%~3.0%, tantalum powder 0.05%~0.15%, yttrium oxide 0.5%~1.5%, cerium oxide 0.2%~0.6%, and the remainder is iron powder. The outer sheath is made of 316 austenitic stainless steel strip, and the core filling rate is 22%-30%.
2. A method for preparing austenitic stainless steel structural components resistant to intergranular corrosion, characterized in that, The powder-cored wire is fused onto the surface of a 316 steel plate using 3D printing technology to obtain austenitic stainless steel structural components resistant to intergranular corrosion; the specific operation steps are as follows: Step 1: Weigh out the following components by mass percentage: graphene 0.07%~0.08%, chromium powder 20.0%~24.0%, nickel powder 15.6%~16.0%, molybdenum powder 4.3%~4.5%, silicon powder 1.2%~2.2%, manganese powder 2.5%~3.5%, titanium powder 1.0%~2.0%, niobium powder 2.0%~3.0%, tantalum powder 0.05%~0.15%, yttrium oxide 0.5%~1.5%, cerium oxide 0.2%~0.6%, with the remainder being iron powder. Mix the weighed alloy powders using a V-type powder mixer to ensure thorough and uniform mixing, then place them in a tube furnace and heat and maintain the temperature in a pure argon atmosphere. The mixing speed of the powder mixer in step 1 is 70 r / min, and the mixing time is 3 h; the heat preservation temperature in step 1 is 200-300℃, and the heat preservation time is 2-2.5 h. Step 2: Wipe the 316 austenitic stainless steel strip with acetone to remove oil stains and dirt from the surface, then put it into an electric resistance furnace and keep it at a temperature of 100-150℃ for 1-1.5 hours to ensure that the surface of the steel strip is smooth. Step 3: Place the austenitic stainless steel strip from Step 2 onto a wire drawing machine, and then roll it into a U-shaped groove through a grooving process. Add the alloy powder obtained in Step 1 into the U-shaped groove of the steel strip. After passing through the closed forming rolls of a fully automatic wire drawing machine, it is made into a 2.30mm welding wire. Finally, it is made into a 1.20mm powder core wire by gradually reducing the diameter. Step 4: Assemble the prepared powder core wire from Step 3 into the fully automatic welding robot. After determining the welding process, plan the welding path and layer height and input them into the welding robot. Select 316 steel plate as the workpiece substrate. Use an angle grinder to remove the oxide scale and impurities on the surface of the steel plate and grind the surface smooth. Then run the welding machine command and use MIG welding as the heat source to 3D print austenitic stainless steel structural parts.
3. The method for preparing intergranular corrosion resistant austenitic stainless steel structural components according to claim 2, characterized in that, The steel strip mentioned in step 2 has a width of 0.7 mm and a thickness of 0.2 mm.
4. The method for preparing intergranular corrosion resistant austenitic stainless steel structural components according to claim 2, characterized in that, In step 4, the austenitic stainless steel structural parts are modeled using 3DS MAX modeling software, and slicing is performed using CAM software.
5. The method for preparing intergranular corrosion resistant austenitic stainless steel structural components according to claim 2, characterized in that, In step 4, the 3D printing process parameters are as follows: cladding voltage is 20.0 V, cladding current is 180.0 A, welding speed is 0.25 m / min; welding swing is 0.8 mm, welding torch is raised 4 mm per layer, shielding gas is 99.99% argon, and gas flow rate is 10~15 L / min.