Preparation method of pole piece edge coating boehmite
By preparing high-purity boehmite and mixing it with a modifier, the problems of discoloration and gelation of boehmite and PVDF when stirred in NMP solvent were solved, thus improving the stability and safety of the electrode edge coating.
Patent Information
- Application Number
- CN202410483688.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-22
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-04-22
AI Technical Summary
When boehmite and PVDF are mixed and NMP solvent is added, red, yellow or gel phenomena are easily produced during high-speed stirring, which makes the slurry difficult to produce and reduces the compressive strength of the electrode, increasing the risk of short circuit.
A method for preparing electrode-side-coated boehmite is adopted, including steps such as dissolving aluminum nitrate nonahydrate, adjusting pH value, hydrothermal reaction, centrifugation sedimentation and vacuum drying, to prepare high-purity boehmite, which is then mixed with a modifier to form a boehmite slurry, avoiding adverse reactions with PVDF and NMP.
The prepared boehmite does not change color or gel after being mixed with PVDF and NMP, ensuring the pressure resistance and safety of the electrode and reducing the risk of short circuit.
Smart Images

Figure CN118373433B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of new material preparation technology, and in particular to a method for preparing boehmite-like electrode edge coatings. Background Technology
[0002] Boehmite (γ-AlOOH) is a major component of bauxite and an important chemical raw material with a unique crystal structure. It is widely used in many fields such as new energy, catalysts and carriers, paper filling materials, and inorganic flame retardants. In particular, with the rapid development of lithium-ion batteries, boehmite has broad application prospects in the fields of separator coating and electrode edge coating.
[0003] The edge reinforcement layer coated on the edge of lithium-ion battery electrode not only enhances the electrode's compressive strength but also reduces the risk of short circuits. The raw materials used in the edge coating are mainly solid powder boehmite, PVDF, and solvent NMP.
[0004] However, after mixing boehmite and PVDF with NMP solvent and stirring at high speed for a certain period of time, the slurry is prone to turning red, yellow, or gelling. This is because the introduction of boehmite can sometimes cause PVDF to deteriorate. Discolored or gelled slurries are not only difficult to produce, but also reduce the compressive strength of the electrode and increase the risk of short circuits. Summary of the Invention
[0005] 1. Technical problems to be solved
[0006] The purpose of this invention is to solve the problem in the prior art that after mixing boehmite and PVDF and adding them to NMP solvent, the slurry is prone to turning red, yellow or gelling after high-speed stirring for a certain period of time. Therefore, this invention proposes a method for preparing boehmite for edge coating of electrodes.
[0007] 2. Technical Solution
[0008] To achieve the above objectives, the present invention adopts the following technical solution:
[0009] A method for preparing boehmite-like electrode edge coating includes the following steps:
[0010] Step 1: Dissolve aluminum nitrate nonahydrate in deionized water to obtain a solution;
[0011] Step 2: Stir the solution from Step 1, add sodium hydroxide solution, and adjust the pH of the solution to 9-12 to obtain a mixture;
[0012] Step 3: Stir the mixture from Step 2 for 1 hour, then centrifuge and collect the gel-like precipitate.
[0013] Step 4: Wash the precipitate obtained in Step 3 with deionized water to remove all soluble salts, and obtain aluminum hydroxide gel;
[0014] Step 5: Dissolve the aluminum hydroxide gel obtained in Step 4 in deionized water to obtain a solution;
[0015] Step 6: Stir the solution from Step 5, add sodium hydroxide solution, and adjust the pH of the solution to 9-12 to obtain a mixed solution;
[0016] Step 7: Perform a hydrothermal reaction on the mixture from Step 6, and collect the gel-like precipitate after centrifugation and sedimentation.
[0017] Step 8: The precipitate obtained in Step 7 is washed and dried to obtain high-purity boehmite;
[0018] Step 9: Add the boehmite obtained in Step 8 and the modifier to an ethanol solvent in a certain proportion to obtain boehmite slurry;
[0019] Step 10: The boehmite slurry obtained in Step 9 is centrifuged, settled, and dried to obtain modified boehmite.
[0020] Preferably, the concentration of the aluminum nitrate nonahydrate solution in step 1 is 0.3-0.6M.
[0021] Preferably, the cleaning process in step 4 is performed three times.
[0022] Preferably, the concentration of the aluminum hydroxide solution in step 5 is 0.3-0.6M.
[0023] Preferably, the stirring time in step 6 is 1 hour.
[0024] Preferably, the reaction temperature in step 7 is 180-250℃ and the reaction time is 2 hours.
[0025] Preferably, the washing process in step 8 is repeated three times; the drying is performed using vacuum drying at a temperature of 60-90℃.
[0026] Preferably, the modifier in step 9 is one or more of silane coupling agents, titanate, and aluminate compounds, with a solid content of 20%, and the mass ratio of boehmite to modifier is 20-40:1.
[0027] Preferably, the drying in step 10 is performed using vacuum drying at a temperature of 70°C.
[0028] This invention also proposes a high-purity boehmite, wherein the boehmite is a white powder with a purity >99.9%, and the boehmite D... 50 The particle size is 0.8-1.5 μm. The boehmite does not change color or gel after being mixed with PVDF and NMP.
[0029] 3. Beneficial effects
[0030] Compared with the prior art, the advantages of this invention are:
[0031] In this invention, the preparation method can effectively prevent discoloration and gelation of PVDF slurry, and can produce high-purity boehmite, which is of great significance for its application in the edge coating of lithium battery positive electrode sheets. Attached Figure Description
[0032] Figure 1 This is a SEM image of the boehmite prepared in Example 1 of the present invention;
[0033] Figure 2 This is a diagram showing the results of mixing boehmite prepared in Example 1 of this invention with PVDF and NMP.
[0034] Figure 3 This is a SEM image of boehmite prepared in Comparative Example 1 of the present invention. Detailed Implementation
[0035] The technical solutions of the present invention will be clearly and completely described below with reference to the accompanying drawings of the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.
[0036] Example 1:
[0037] A method for preparing boehmite-like electrode edge coating includes the following steps:
[0038] Step 1: Dissolve aluminum nitrate nonahydrate in deionized water to obtain an aluminum nitrate nonahydrate solution with a concentration of 0.5M;
[0039] Step 2: Stir the solution from Step 1, add sodium hydroxide solution, and adjust the pH of the solution to 12 to obtain a mixture;
[0040] Step 3: Stir the mixture from Step 2 for 1 hour, then centrifuge and collect the gel-like precipitate.
[0041] Step 4: Wash the precipitate obtained in Step 3 with deionized water three times to obtain aluminum hydroxide gel;
[0042] Step 5: Dissolve the aluminum hydroxide gel obtained in Step 4 in deionized water to obtain an aluminum hydroxide solution with a concentration of 0.5M;
[0043] Step 6: Stir the solution from Step 5 for 1 hour, add sodium hydroxide solution, and adjust the pH of the solution to 12 to obtain a mixture;
[0044] Step 7: The mixture from Step 6 is subjected to a hydrothermal reaction at a temperature of 200°C for 2 hours. After centrifugation and sedimentation, the gel-like precipitate is collected.
[0045] Step 8: Wash the precipitate obtained in Step 7 with deionized water three times, and then vacuum dry it at 80°C for 6 hours to obtain boehmite.
[0046] Step 9: Add the boehmite obtained in Step 8 and the silane coupling agent to an ethanol solvent at a mass ratio of 20:1 and a solid content of 20% to obtain a boehmite slurry;
[0047] Step 10: The boehmite slurry obtained in Step 9 is centrifuged and then vacuum dried at 70°C for 8 hours to obtain modified boehmite;
[0048] In this embodiment, the prepared boehmite is a white powder with a purity of 99.94%, D 50 The sample had a particle size of 1.1 μm. Boehmite was mixed with PVDF and NMP at a mass ratio of 28:4:68, and the mixture was stirred at 1000 rpm for 4 hours. After this mixture, it did not change color or gel. SEM images of the boehmite prepared in this example are shown below. Figure 1 As shown, after mixing with PVDF and NMP, the following results were observed. Figure 2 As shown in the right cup.
[0049] Example 2:
[0050] It has the implementation content of the above embodiments, wherein the specific implementation of the above embodiments can be referred to the above description, and the embodiments here will not be repeated in detail; however, the difference between this application embodiment and the above embodiments is that the deionized water rinsing in step 4 is changed to once.
[0051] The boehmite prepared in this embodiment was tested and found to be a white powder with a purity of 99.73%. 50 The sample was 1.2 μm thick. Boehmite was mixed with PVDF and NMP at a mass ratio of 28:4:68 and a rotation speed of 1000 rpm for 4 hours. The mixture did not change color or gel.
[0052] Example 3:
[0053] It has the implementation content of the above embodiments, wherein the specific implementation of the above embodiments can be referred to the above description, and the embodiments here will not be repeated in detail; however, the difference between the present application embodiment and the above embodiments is that the reaction temperature in step 7 is changed to 180°C.
[0054] The boehmite prepared in this embodiment was tested and found to be a white powder with a purity of 99.81%. 50The particle size was 0.8 μm. Boehmite was mixed with PVDF and NMP at a mass ratio of 28:4:68 and the mixing speed was 1000 rpm. After 4 hours of mixing, the mixture did not change color or gel.
[0055] Example 4:
[0056] It has the implementation content of the above embodiments, wherein the specific implementation of the above embodiments can be referred to the above description, and the embodiments here will not be repeated in detail; however, the difference between the present application embodiment and the above embodiments is that the reaction temperature in step 7 is changed to 250°C.
[0057] The boehmite prepared in this embodiment was tested and found to be a white powder with a purity of 99.93%. 50 The sample was 1.6 μm thick. Boehmite was mixed with PVDF and NMP at a mass ratio of 28:4:68 and a rotation speed of 1000 rpm for 4 hours. The mixture did not change color or gel.
[0058] Example 5:
[0059] It has the implementation content of the above embodiments, wherein the specific implementation of the above embodiments can be referred to the above description, and the embodiments here will not be repeated in detail; however, the difference between the embodiments in this application and the above embodiments is that the mass ratio of boehmite to silane coupling agent in step 9 is changed to 40:1.
[0060] The boehmite prepared in this embodiment was tested and found to be a white powder with a purity of 99.94%. 50 The sample was 1.1 μm thick. Boehmite was mixed with PVDF and NMP at a mass ratio of 28:4:68 and a rotation speed of 1000 rpm for 4 hours. The mixture did not change color or gel.
[0061] Example 6:
[0062] It has the implementation content of the above embodiments, wherein the specific implementation of the above embodiments can be referred to the above description, and the embodiments here will not be repeated in detail; however, the difference between the present application embodiment and the above embodiments is that: in step 9, the modifier is replaced with phthalate ester.
[0063] The boehmite prepared in this embodiment was tested and found to be a white powder with a purity of 99.90%. 50 The sample was 1.0 μm thick. Boehmite was mixed with PVDF and NMP at a mass ratio of 28:4:68 and the mixture was stirred at 1000 rpm for 4 hours. The mixture did not change color or gel.
[0064] Example 7:
[0065] It has the implementation content of the above embodiments, wherein the specific implementation of the above embodiments can be referred to the above description, and the embodiments here will not be repeated in detail; however, the difference between the present application embodiment and the above embodiments is that: in step 9, the modifier is replaced with an aluminate compound.
[0066] The boehmite prepared in this embodiment was tested and found to be a white powder with a purity of 99.91%. 50 The sample was 1.3 μm thick. Boehmite was mixed with PVDF and NMP at a mass ratio of 28:4:68 and a rotation speed of 1000 rpm for 4 hours. The mixture did not change color or gel.
[0067] Comparative Example 1:
[0068] It has the implementation content of the above embodiments, wherein the specific implementation methods of the above embodiments can be referred to the above description, and the embodiments here will not be described in detail again; however, the difference between the embodiments in this application and the above embodiments is that steps 9 and 10 are not performed.
[0069] The boehmite prepared in this embodiment was tested and found to be a white powder with a purity of 99.93%. 50 The sample had a particle size of 0.9 μm. Boehmite was mixed with PVDF and NMP at a mass ratio of 28:4:68, and the mixture was stirred at 1000 rpm for 4 hours. After mixing, the mixture turned yellow and formed a gel. SEM images of the boehmite prepared in this example are shown below. Figure 3 As shown, after mixing with PVDF and NMP, the following results were observed. Figure 2 As shown in the left cup
[0070] Comparative Example 2:
[0071] It has the implementation content of the above embodiments, wherein the specific implementation of the above embodiments can be referred to the above description, and the embodiments here will not be repeated in detail; however, the difference between the embodiments in this application and the above embodiments is that the mass ratio of boehmite to silane coupling agent in step 9 is changed to 50:1.
[0072] The boehmite prepared in this embodiment was tested and found to be a white powder with a purity of 99.90%. 50 The sample was 1.1 μm thick. Boehmite was mixed with PVDF and NMP at a mass ratio of 28:4:68 and rotated at 1000 rpm for 4 hours. The mixture turned yellow and formed a gel.
[0073] The above description is only a preferred embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any equivalent substitutions or modifications made by those skilled in the art within the scope of the technology disclosed in the present invention, based on the technical solution and inventive concept of the present invention, should be covered within the scope of protection of the present invention.
Claims
1. A method for preparing boehmite-like coatings on electrode edges, characterized in that, Includes the following steps: Step 1: Dissolve aluminum nitrate nonahydrate in deionized water to obtain a solution; Step 2: Stir the solution from Step 1, add sodium hydroxide solution, and adjust the pH of the solution to 9-12 to obtain a mixture; Step 3: Stir the mixture from Step 2 for 1 hour, then centrifuge and collect the gel-like precipitate. Step 4: Wash the precipitate obtained in Step 3 with deionized water to remove all soluble salts, and obtain aluminum hydroxide gel; Step 5: Dissolve the aluminum hydroxide gel obtained in Step 4 in deionized water to obtain a solution; Step 6: Stir the solution from Step 5, add sodium hydroxide solution, and adjust the pH of the solution to 9-12 to obtain a mixed solution; Step 7: Perform a hydrothermal reaction on the mixture from Step 6, and collect the gel-like precipitate after centrifugation and sedimentation. In step 7, the reaction temperature is 180-250℃ and the reaction time is 2 hours. Step 8: The precipitate obtained in Step 7 is washed and dried to obtain high-purity boehmite; Step 9: Add the boehmite obtained in Step 8 and the modifier to an ethanol solvent in a certain proportion to obtain boehmite slurry; In step 9, the modifier is one or more of silane coupling agents, titanate, and aluminate compounds, with a solid content of 20% and a mass ratio of boehmite to modifier of 20-40:
1. Step 10: The boehmite slurry obtained in Step 9 is centrifuged, settled, and dried to obtain modified boehmite.
2. The method for preparing an electrode edge-coated boehmite according to claim 1, characterized in that, In step 1, the concentration of aluminum nitrate nonahydrate solution is 0.3-0.6M.
3. The method for preparing an electrode edge-coated boehmite according to claim 1, characterized in that, The cleaning process in step 4 involves three cycles.
4. The method for preparing an electrode edge-coated boehmite according to claim 1, characterized in that, In step 5, the concentration of the aluminum hydroxide solution is 0.3-0.6M.
5. The method for preparing an electrode edge-coated boehmite according to claim 1, characterized in that, The stirring time in step 6 is 1 hour.
6. The method for preparing an electrode edge-coated boehmite according to claim 1, characterized in that, In step 8, the cleaning is performed 3 times; the drying is carried out using vacuum drying at a temperature of 60-90℃.
7. The method for preparing an electrode edge-coated boehmite according to claim 1, characterized in that, In step 10, the drying process is performed using vacuum drying at a temperature of 70°C.
8. The high-purity boehmite prepared by any one of the preparation methods according to claims 1-7, characterized in that, The boehmite is a white powder with a purity >99.9%, and the boehmite D 50 The particle size is 0.8-1.5 μm. The boehmite does not change color or gel after being mixed with PVDF and NMP.
Citation Information
Patent Citations
Preparation method of boehmite with low water absorption
CN112456525A
Production of high purity pseudo-boehmite powder
JP1996268715A
Preparation method of transparent alumina sols
KR1020120057922A