Phosphate optical glass and process for producing the same

By adjusting the component ratio of phosphate optical glass and using efficient mixing equipment, the problem of low raw material mixing efficiency was solved, and optical glass that meets high requirements was prepared, achieving high stability and high transmittance.

CN118373590BActive Publication Date: 2026-11-24SHANGHAI TAIYANG TECHNOLOGY CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410458226.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-16
Publication Date
2026-11-24
Estimated Expiration
2044-04-16

AI Technical Summary

Technical Problem

In the existing process of preparing phosphate optical glass, the raw material mixing efficiency is low, and it is difficult to obtain optical glass with high stability and visible light transmittance, especially products with refractive index and Abbe number within a specific range.

Method used

The component ratio of phosphate optical glass is adjusted, and raw material mixing equipment is used, combined with the first and second stirring mechanisms to carry out counter- and co-directional stirring, thereby improving the mixing efficiency. The glass is then melted at high temperature in a quartz ceramic crucible and clarified to reduce the melting temperature and improve the stability and transmittance of the glass.

Benefits of technology

Efficient mixing was achieved to prepare phosphate optical glass with a refractive index of 1.94-1.96 and an Abbe number of 23-24. It has excellent transmittance, chemical stability and mechanical properties, and is suitable for high-requirement optical lenses.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118373590B_ABST
    Figure CN118373590B_ABST
Patent Text Reader

Abstract

This invention relates to the field of glass manufacturing technology, specifically to a phosphate optical glass comprising the following raw materials in the indicated weight ratios: 35-45 parts aluminum metaphosphate, 18-23 parts barium metaphosphate, 8-22 parts phosphorus pentoxide, 3-7 parts niobium pentoxide, 0.5-1.5 parts antimony trioxide, 5-15 parts tungsten oxide, 6-10 parts titanium oxide, 4-10 parts sodium oxide, and 5-9 parts zirconium dioxide. This invention prepares phosphate optical glass by effectively lowering the melting temperature of the glass raw materials through the addition of phosphorus pentoxide. Furthermore, its combination with other raw material components improves the stability and visible light transmittance of the glass, resulting in low relative partial dispersion, excellent transmittance, chemical stability, and mechanical properties. It can be used in the field of optical glass where high-performance lenses are required. The glass preparation process utilizes a raw material mixing device to achieve efficient mixing, facilitating mass production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of glass production technology, specifically to a phosphate optical glass and its preparation process. Background Technology

[0002] The rapid development of new optoelectronic products has created a significant demand for optical glass with a refractive index range of 1.93-1.95 and an Abbe number range of 20-30. Based on the relationship between refractive index and Abbe number, the SiO2-Nb2O5-TiO2-BaO-R2O formulation system is unsuitable for optical glass with a refractive index range of 1.93-1.95 and an Abbe number range of 20-30. This is because the glass system becomes extremely unstable in this configuration, making it difficult to obtain products with uniform internal quality requirements. Furthermore, the transmittance and chemical stability (primarily due to SiO2's poor fluorine resistance) are also unsatisfactory. Using a phosphate formulation system can provide significant stability to the glass while ensuring visible light transmittance.

[0003] A search revealed Chinese Patent Publication No. CN108675631B, which discloses a phosphate optical glass, its preparation method, and optical elements and filters. The phosphate optical glass, by elemental mass percentage, comprises: P: 12-45%, B: 0-6%, Si: 0.1-6%, Al: 1-15%, O: 42.5-60%, Fe: 0.5-6%, R: 1-10%, R′: 0.1-3%, where R is one or a combination of Mg, Ca, Sr, and Ba, and R′ is Na and / or K. The phosphate optical glass does not contain Pb, Cd, or As. The prepared phosphate optical glass exhibits excellent visible light transmittance and near-infrared light absorption characteristics. Furthermore, it demonstrates good chemical stability and excellent mass production processing performance, making it suitable for manufacturing optical elements and filters that absorb near-infrared light.

[0004] The applicant previously disclosed a phosphate optical glass and its preparation method in patent CN116239301B. The components, expressed in parts by weight, are: 40-50 parts La+Y doped aluminum metaphosphate, 22-25 parts barium metaphosphate, 5-15 parts tungsten oxide, 6-10 parts titanium oxide, and 10-30 parts phosphorus pentoxide. The raw materials for the prepared phosphate optical glass are widely available and low in cost. The resulting phosphate optical glass exhibits good light transmission properties, with a refractive index of 1.96-1.98, an Abbe number of 25-26, a crystallization upper limit temperature below 1100℃, and low relative partial dispersion. It can be applied in optical glass fields such as mobile phones and cameras where high-performance lenses are required, and can reduce residual chromatic aberration in the secondary spectrum. However, the preparation of the aforementioned La+Y doped aluminum metaphosphate requires complex steps such as sol preparation, aging to obtain a gel, drying, calcination, and grinding; and the mixing efficiency is low during the mixing step. In view of this, we propose a phosphate optical glass and its preparation method. Summary of the Invention

[0005] The purpose of this invention is to provide a phosphate optical glass and its preparation process, which adjusts the glass components and component ratios, and uses a raw material mixing device to improve mixing efficiency, thereby solving the problems mentioned in the background art.

[0006] To achieve the above objectives, the present invention provides the following technical solution:

[0007] A phosphate optical glass comprises the following raw materials in the indicated weight ratios: 35-45 parts aluminum metaphosphate, 18-23 parts barium metaphosphate, 8-22 parts phosphorus pentoxide, 3-7 parts niobium pentoxide, 0.5-1.5 parts antimony trioxide, 5-15 parts tungsten oxide, 6-10 parts titanium oxide, 4-10 parts sodium oxide, and 5-9 parts zirconium dioxide.

[0008] A process for preparing phosphate optical glass includes the following steps:

[0009] S1. Weigh the raw materials such as aluminum metaphosphate, barium metaphosphate, phosphorus pentoxide, niobium pentoxide, antimony trioxide, tungsten oxide, titanium oxide, sodium oxide and zirconium dioxide according to the proportion using a weighing device, and set the weighed raw materials aside.

[0010] S2. The prepared raw materials such as aluminum metaphosphate, barium metaphosphate, phosphorus pentoxide, niobium pentoxide, antimony trioxide, tungsten oxide, titanium oxide, sodium oxide and zirconium dioxide are measured and mixed using a raw material mixing device to ensure that the raw materials are mixed evenly.

[0011] S3. Place the evenly mixed raw materials into a quartz ceramic crucible and perform initial melting. Raise the temperature to a high temperature for melting, stirring and homogenizing during the process. After stirring, raise the temperature to 1360-1420℃ and keep it at that temperature for 5-10 hours to clarify the material and allow the bubbles to rise fully. After the raw materials have melted into glass liquid, cool them down.

[0012] S4. After melting is complete, pour or strain the molten glass into a preheated mold to form it, and then place the formed glass in an annealing furnace for annealing.

[0013] Preferably, the phosphate optical glass has a refractive index in the range of 1.94-1.96 and an Abbe number in the range of 23-24.

[0014] Preferably, the initial melting temperature in the quartz ceramic crucible during step S3 is between 1150℃ and 1250℃.

[0015] Preferably, the stirring time in step S3 is controlled at 2.5-6 hours.

[0016] Preferably, the temperature of the cooling process in step S3 is reduced to the range of 1050-1200℃.

[0017] A raw material mixing device includes a barrel body, a first stirring mechanism, and a second stirring mechanism. A barrel cover is fixedly installed on the barrel body. The first stirring mechanism is located inside the barrel body, and the second stirring mechanism is located inside the barrel body.

[0018] Specifically, by setting up a first stirring mechanism and a second stirring mechanism, the raw materials inside the tank can be stirred in opposite directions and in the same direction, thereby improving the stirring effect of the raw materials.

[0019] The first stirring mechanism includes a first stirring motor and a rotating shaft. The rotating shaft is fixedly installed on the output end of the first stirring motor. A base frame is fixedly installed on the lower end of the rotating shaft. A fixing column is fixedly installed on the base frame. A first stirring blade is fixedly installed on the fixing column.

[0020] Specifically, the first stirring motor drives the rotating shaft to rotate, thereby causing the first stirring blades to stir the raw materials inside the tank.

[0021] The second stirring mechanism includes a second stirring motor and a rotating drum. A first transmission wheel is fixedly installed on the output end of the second stirring motor, and a belt is driven to the first transmission wheel. A second transmission wheel is fixedly installed on the rotating drum, and the belt is driven to the second transmission wheel.

[0022] Specifically, by starting the second stirring motor, it drives the first transmission wheel, belt and second transmission wheel to run, thereby driving the rotating drum to rotate, and the second stirring blades on the rotating drum to stir and mix the raw materials inside the drum.

[0023] A second stirring blade is fixedly installed on the rotating drum, a first bearing is fixedly installed on the drum cover, the rotating drum is fixedly installed on the inner wall of the inner ring of the first bearing, a second bearing is fixedly installed on the inner wall of the rotating drum, and the rotating shaft is fixedly installed on the inner wall of the inner ring of the second bearing.

[0024] Specifically, the second bearing allows the shaft to rotate inside the drum, thus ensuring that the rotation of the shaft does not affect the rotation of the drum.

[0025] A motor frame is fixedly installed on the upper surface of the barrel lid. The first stirring motor is fixedly installed on the motor frame, and the second stirring motor is fixedly installed on the motor frame. A feed inlet is provided on the barrel lid.

[0026] The bottom of the barrel has a discharge port, and support legs are fixedly installed on the outer wall of the barrel.

[0027] Specifically, the motor frame allows for easy mounting of the first and second stirring motors on the lid, while the support legs provide support for the container.

[0028] Compared with the prior art, the beneficial effects of the present invention are:

[0029] 1. The raw materials required for preparing phosphate optical glass according to this invention are widely available and low in cost. By adding phosphorus pentoxide, the melting temperature of the glass raw material can be effectively reduced. Furthermore, when used in combination with other raw material components, the stability and visible light transmittance of the glass can be improved, resulting in optical glass with a refractive index of 1.94-1.96 and an Abbe number of 23-24. It has low relative partial dispersion, excellent transmittance, chemical stability, and mechanical properties, and can be used in the field of optical glass with high requirements for optical lenses.

[0030] 2. The phosphate optical glass and its preparation process, by setting up a first stirring mechanism and a second stirring mechanism, can perform counter-directional and co-directional stirring of the raw materials inside the barrel, thereby improving the stirring effect of the raw materials. The first stirring motor drives the rotating shaft to rotate, so that the first stirring blades stir the raw materials inside the barrel. By starting the second stirring motor, it drives the first transmission wheel, belt and second transmission wheel to run, thereby driving the rotating drum to rotate, so that the second stirring blades on the rotating drum stir and mix the raw materials inside the barrel. When counter-directional stirring is required, the two motors can be controlled to rotate clockwise and counter-clockwise respectively to achieve the purpose of cross stirring. When co-directional stirring is required, the two motors can be controlled to rotate in the same direction. Adjusting the speed of the motors can achieve the purpose of staggered stirring, thereby improving the mixing effect of the raw materials and realizing efficient mixing. Attached Figure Description

[0031] Figure 1 This is a schematic diagram of the preparation process of the present invention;

[0032] Figure 2 This is a schematic diagram of the raw material mixing equipment of the present invention;

[0033] Figure 3 This is a schematic diagram of the internal structure of the barrel of the present invention;

[0034] Figure 4 This is a schematic diagram of the cross-sectional structure of the rotating cylinder of the present invention;

[0035] Figure 5 This is a schematic diagram of the first stirring mechanism of the present invention;

[0036] Figure 6 This is a schematic diagram of the second stirring mechanism of the present invention;

[0037] Figure 7 For the present invention Figure 4 Enlarged schematic diagram of the structure at point A in the middle.

[0038] In the diagram: 1. Barrel body; 2. First stirring mechanism; 201. First stirring motor; 202. Rotating shaft; 203. Base frame; 204. Fixed column; 205. First stirring blade; 3. Second stirring mechanism; 301. Second stirring motor; 302. First transmission wheel; 303. Belt; 304. Second transmission wheel; 305. First bearing; 306. Rotating drum; 307. Second stirring blade; 308. Second bearing; 4. Barrel lid; 5. Support leg; 6. Feed inlet; 7. Discharge outlet; 8. Motor frame. Detailed Implementation

[0039] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0040] In the description of this invention, it should be understood that the terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," and "counterclockwise," etc., indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.

[0041] In the description of this invention, it should be noted that, unless otherwise explicitly specified and limited, the terms "installation," "connection," "linking," and "setting" should be interpreted broadly. For example, they can refer to a fixed connection or setting, a detachable connection or setting, or an integral connection or setting. Those skilled in the art can understand the specific meaning of the above terms in this patent according to the specific circumstances.

[0042] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include one or more of that feature. In the description of this invention, "a number" means two or more, unless otherwise explicitly specified.

[0043] The applicant previously disclosed a phosphate optical glass and its preparation method in patent CN116239301B. The preparation of the La+Y doped aluminum metaphosphate requires complex steps such as sol preparation, aging to obtain a gel, drying, calcination, and grinding; and the mixing efficiency is low during the mixing step. Therefore, we propose a phosphate optical glass and its preparation process.

[0044] Example 1

[0045] like Figure 1 As shown, a phosphate optical glass comprises the following raw materials in the indicated weight ratios: 35 parts aluminum metaphosphate, 18 parts barium metaphosphate, 8 parts phosphorus pentoxide, 3 parts niobium pentoxide, 0.5 parts antimony trioxide, 5 parts tungsten oxide, 6 parts titanium oxide, 4 parts sodium oxide, and 5 parts zirconium dioxide.

[0046] A process for preparing phosphate optical glass includes the following steps:

[0047] S1. Weigh the raw materials such as aluminum metaphosphate, barium metaphosphate, phosphorus pentoxide, niobium pentoxide, antimony trioxide, tungsten oxide, titanium oxide, sodium oxide and zirconium dioxide according to the proportion using a weighing device, and set the weighed raw materials aside.

[0048] S2. The prepared raw materials such as aluminum metaphosphate, barium metaphosphate, phosphorus pentoxide, niobium pentoxide, antimony trioxide, tungsten oxide, titanium oxide, sodium oxide and zirconium dioxide are measured and mixed using a raw material mixing device to ensure that the raw materials are mixed evenly.

[0049] S3. Place the uniformly mixed raw materials into a quartz ceramic crucible and perform initial melting. Raise the temperature to a high temperature for melting, stirring and homogenizing during the process. Control the stirring time to 2.5-6 hours. After stirring, raise the temperature to 1360-1420℃ and hold for 5-10 hours to clarify, allowing the bubbles to rise fully. After the raw materials have melted into glass liquid, cool them down.

[0050] The initial melting temperature in the quartz ceramic crucible is between 1150℃ and 1250℃, and the cooling treatment temperature is reduced to the range of 1050-1200℃.

[0051] S4. After melting is complete, pour or strain the molten glass into a preheated mold to form it, and then place the formed glass in an annealing furnace for annealing.

[0052] Example 2

[0053] like Figure 1 As shown, a phosphate optical glass comprises the following raw materials in the indicated weight ratios: 45 parts aluminum metaphosphate, 23 parts barium metaphosphate, 22 parts phosphorus pentoxide, 7 parts niobium pentoxide, 1.5 parts antimony trioxide, 15 parts tungsten oxide, 10 parts titanium oxide, 10 parts sodium oxide, and 9 parts zirconium dioxide.

[0054] A process for preparing phosphate optical glass includes the following steps:

[0055] S1. Weigh the raw materials such as aluminum metaphosphate, barium metaphosphate, phosphorus pentoxide, niobium pentoxide, antimony trioxide, tungsten oxide, titanium oxide, sodium oxide and zirconium dioxide according to the proportion using a weighing device, and set the weighed raw materials aside.

[0056] S2. The prepared raw materials such as aluminum metaphosphate, barium metaphosphate, phosphorus pentoxide, niobium pentoxide, antimony trioxide, tungsten oxide, titanium oxide, sodium oxide and zirconium dioxide are measured and mixed using a raw material mixing device to ensure that the raw materials are mixed evenly.

[0057] S3. Place the uniformly mixed raw materials into a quartz ceramic crucible and perform initial melting. Raise the temperature to a high temperature for melting, stirring and homogenizing during the process. Control the stirring time to 2.5-6 hours. After stirring, raise the temperature to 1360-1420℃ and hold for 5-10 hours to clarify, allowing the bubbles to rise fully. After the raw materials have melted into glass liquid, cool them down.

[0058] The initial melting temperature in the quartz ceramic crucible is between 1150℃ and 1250℃, and the cooling treatment temperature is reduced to the range of 1050-1200℃.

[0059] S4. After melting is complete, pour or strain the molten glass into a preheated mold to form it, and then place the formed glass in an annealing furnace for annealing.

[0060] Example 3

[0061] like Figure 1 As shown, a phosphate optical glass comprises the following raw materials in the indicated weight ratios: 37 parts aluminum metaphosphate, 20 parts barium metaphosphate, 8 parts phosphorus pentoxide, 7 parts niobium pentoxide, 0.5 parts antimony trioxide, 15 parts tungsten oxide, 6 parts titanium oxide, 10 parts sodium oxide, and 5 parts zirconium dioxide.

[0062] A process for preparing phosphate optical glass includes the following steps:

[0063] S1. Weigh the raw materials such as aluminum metaphosphate, barium metaphosphate, phosphorus pentoxide, niobium pentoxide, antimony trioxide, tungsten oxide, titanium oxide, sodium oxide and zirconium dioxide according to the proportion using a weighing device, and set the weighed raw materials aside.

[0064] S2. The prepared raw materials such as aluminum metaphosphate, barium metaphosphate, phosphorus pentoxide, niobium pentoxide, antimony trioxide, tungsten oxide, titanium oxide, sodium oxide and zirconium dioxide are measured and mixed using a raw material mixing device to ensure that the raw materials are mixed evenly.

[0065] S3. Place the uniformly mixed raw materials into a quartz ceramic crucible and perform initial melting. Raise the temperature to a high temperature for melting, stirring and homogenizing during the process. Control the stirring time to 2.5-6 hours. After stirring, raise the temperature to 1360-1420℃ and hold for 5-10 hours to clarify, allowing the bubbles to rise fully. After the raw materials have melted into glass liquid, cool them down.

[0066] The initial melting temperature in the quartz ceramic crucible is between 1150℃ and 1250℃, and the cooling treatment temperature is reduced to the range of 1050-1200℃.

[0067] S4. After melting is complete, pour or strain the molten glass into a preheated mold to form it, and then place the formed glass in an annealing furnace for annealing.

[0068] Example 4

[0069] like Figure 1 As shown, a phosphate optical glass comprises the following raw materials in the indicated weight ratios: 40 parts aluminum metaphosphate, 22 parts barium metaphosphate, 19 parts phosphorus pentoxide, 5 parts niobium pentoxide, 1 part antimony trioxide, 10 parts tungsten oxide, 7 parts titanium oxide, 4 parts sodium oxide, and 6 parts zirconium dioxide.

[0070] A process for preparing phosphate optical glass includes the following steps:

[0071] S1. Weigh the raw materials such as aluminum metaphosphate, barium metaphosphate, phosphorus pentoxide, niobium pentoxide, antimony trioxide, tungsten oxide, titanium oxide, sodium oxide and zirconium dioxide according to the proportion using a weighing device, and set the weighed raw materials aside.

[0072] S2. The prepared raw materials such as aluminum metaphosphate, barium metaphosphate, phosphorus pentoxide, niobium pentoxide, antimony trioxide, tungsten oxide, titanium oxide, sodium oxide and zirconium dioxide are measured and mixed using a raw material mixing device to ensure that the raw materials are mixed evenly.

[0073] S3. Place the uniformly mixed raw materials into a quartz ceramic crucible and perform initial melting. Raise the temperature to a high temperature for melting, stirring and homogenizing during the process. Control the stirring time to 2.5-6 hours. After stirring, raise the temperature to 1360-1420℃ and hold for 5-10 hours to clarify, allowing the bubbles to rise fully. After the raw materials have melted into glass liquid, cool them down.

[0074] The initial melting temperature in the quartz ceramic crucible is between 1150℃ and 1250℃, and the cooling treatment temperature is reduced to the range of 1050-1200℃.

[0075] S4. After melting is complete, pour or strain the molten glass into a preheated mold to form it, and then place the formed glass in an annealing furnace for annealing.

[0076] Example 5

[0077] like Figure 1 As shown, a phosphate optical glass comprises the following raw materials in the indicated weight ratios: 35 parts aluminum metaphosphate, 20 parts barium metaphosphate, 11 parts phosphorus pentoxide, 3 parts niobium pentoxide, 0.8 parts antimony trioxide, 5 parts tungsten oxide, 6 parts titanium oxide, 4 parts sodium oxide, and 5 parts zirconium dioxide.

[0078] A process for preparing phosphate optical glass includes the following steps:

[0079] S1. Weigh the raw materials such as aluminum metaphosphate, barium metaphosphate, phosphorus pentoxide, niobium pentoxide, antimony trioxide, tungsten oxide, titanium oxide, sodium oxide and zirconium dioxide according to the proportion using a weighing device, and set the weighed raw materials aside.

[0080] S2. The prepared raw materials such as aluminum metaphosphate, barium metaphosphate, phosphorus pentoxide, niobium pentoxide, antimony trioxide, tungsten oxide, titanium oxide, sodium oxide and zirconium dioxide are measured and mixed using a raw material mixing device to ensure that the raw materials are mixed evenly.

[0081] S3. Place the uniformly mixed raw materials into a quartz ceramic crucible and perform initial melting. Raise the temperature to a high temperature for melting, stirring and homogenizing during the process. Control the stirring time to 2.5-6 hours. After stirring, raise the temperature to 1360-1420℃ and hold for 5-10 hours to clarify, allowing the bubbles to rise fully. After the raw materials have melted into glass liquid, cool them down.

[0082] The initial melting temperature in the quartz ceramic crucible is between 1150℃ and 1250℃, and the cooling treatment temperature is reduced to the range of 1050-1200℃.

[0083] S4. After melting is complete, pour or strain the molten glass into a preheated mold to form it, and then place the formed glass in an annealing furnace for annealing.

[0084] Example 6

[0085] like Figure 1 As shown, a phosphate optical glass comprises the following raw materials in the indicated weight ratios: 40 parts aluminum metaphosphate, 18 parts barium metaphosphate, 17 parts phosphorus pentoxide, 7 parts niobium pentoxide, 1.5 parts antimony trioxide, 5 parts tungsten oxide, 10 parts titanium oxide, 4 parts sodium oxide, and 5 parts zirconium dioxide.

[0086] A process for preparing phosphate optical glass includes the following steps:

[0087] S1. Weigh the raw materials such as aluminum metaphosphate, barium metaphosphate, phosphorus pentoxide, niobium pentoxide, antimony trioxide, tungsten oxide, titanium oxide, sodium oxide and zirconium dioxide according to the proportion using a weighing device, and set the weighed raw materials aside.

[0088] S2. The prepared raw materials such as aluminum metaphosphate, barium metaphosphate, phosphorus pentoxide, niobium pentoxide, antimony trioxide, tungsten oxide, titanium oxide, sodium oxide and zirconium dioxide are measured and mixed using a raw material mixing device to ensure that the raw materials are mixed evenly.

[0089] S3. Place the uniformly mixed raw materials into a quartz ceramic crucible and perform initial melting. Raise the temperature to a high temperature for melting, stirring and homogenizing during the process. Control the stirring time to 2.5-6 hours. After stirring, raise the temperature to 1360-1420℃ and hold for 5-10 hours to clarify, allowing the bubbles to rise fully. After the raw materials have melted into glass liquid, cool them down.

[0090] The initial melting temperature in the quartz ceramic crucible is between 1150℃ and 1250℃, and the cooling treatment temperature is reduced to the range of 1050-1200℃.

[0091] S4. After melting is complete, pour or strain the molten glass into a preheated mold to form it, and then place the formed glass in an annealing furnace for annealing.

[0092] Example 7

[0093] like Figure 2-7 As shown, the present invention also provides a raw material mixing device, including a barrel body 1, a first stirring mechanism 2 and a second stirring mechanism 3. A barrel cover 4 is fixedly installed on the barrel body 1. The first stirring mechanism 2 is disposed inside the barrel body 1, and the second stirring mechanism 3 is disposed inside the barrel body 1.

[0094] Specifically, by setting up the first stirring mechanism 2 and the second stirring mechanism 3, the raw materials inside the barrel 1 can be stirred in opposite directions and in the same direction, thereby improving the stirring effect of the raw materials.

[0095] like Figure 2-5 As shown, the first stirring mechanism 2 includes a first stirring motor 201 and a rotating shaft 202. The rotating shaft 202 is fixedly installed on the output end of the first stirring motor 201. A base frame 203 is fixedly installed on the lower end of the rotating shaft 202. A fixing column 204 is fixedly installed on the base frame 203. A first stirring blade 205 is fixedly installed on the fixing column 204.

[0096] Specifically, the first stirring motor 201 drives the rotating shaft 202 to rotate, thereby causing the first stirring blades 205 to stir the raw materials inside the barrel 1.

[0097] like Figure 2 , 3 As shown in Figures 4 and 6, the second stirring mechanism 3 includes a second stirring motor 301 and a rotating drum 306. A first transmission wheel 302 is fixedly installed on the output end of the second stirring motor 301. A belt 303 is driven to the first transmission wheel 302. A second transmission wheel 304 is fixedly installed on the rotating drum 306. The belt 303 is driven to the second transmission wheel 304.

[0098] Specifically, by starting the second stirring motor 301, it drives the first transmission wheel 302, belt 303 and second transmission wheel 304 to run, thereby driving the rotating drum 306 to rotate, and the second stirring blades 307 on the rotating drum 306 to stir and mix the raw materials inside the barrel 1.

[0099] A second stirring blade 307 is fixedly installed on the rotating drum 306, a first bearing 305 is fixedly installed on the barrel cover 4, the rotating drum 306 is fixedly installed on the inner wall of the inner ring of the first bearing 305, a second bearing 308 is fixedly installed on the inner wall of the rotating drum 306, and the rotating shaft 202 is fixedly installed on the inner wall of the inner ring of the second bearing 308.

[0100] Specifically, the second bearing 308 allows the rotating shaft 202 to rotate inside the rotating drum 306, thus ensuring that the rotation of the rotating shaft 202 does not affect the rotation of the rotating drum 306.

[0101] like Figure 1 , 2 As shown, a motor frame 8 is fixedly installed on the upper surface of the bucket lid 4, a first stirring motor 201 is fixedly installed on the motor frame 8, a second stirring motor 301 is fixedly installed on the motor frame 8, and a feed inlet 6 is provided on the bucket lid 4.

[0102] The bottom of the barrel 1 is provided with a discharge port 7, and a support leg 5 is fixedly installed on the outer wall of the barrel 1.

[0103] Specifically, the motor frame 8 allows the first stirring motor 201 and the second stirring motor 301 to be conveniently mounted on the lid 4, and the supporting legs 5 provide support for the body 1.

[0104] By setting up a first stirring mechanism 2 and a second stirring mechanism 3, the raw materials inside the barrel 1 can be stirred in opposite directions and in the same direction, improving the stirring effect of the raw materials. The first stirring motor 201 drives the rotating shaft 202 to rotate, so that its first stirring blade 205 stirs the raw materials inside the barrel 1. By starting the second stirring motor 301, it drives the first transmission wheel 302, belt 303 and second transmission wheel 304 to run, thereby driving the rotating drum 306 to rotate, so that the second stirring blade 307 on the rotating drum 306 stirs and mixes the raw materials inside the barrel 1. When opposite stirring is required, the two motors can be controlled to rotate clockwise and counterclockwise respectively to achieve the purpose of cross stirring. When in the same direction stirring is required, the two motors can be controlled to rotate in the same direction. Adjusting the speed of the motors can achieve the purpose of staggered stirring, improving the mixing effect of the raw materials and realizing efficient mixing.

[0105] The raw materials required for preparing phosphate optical glass in this invention are widely available and low in cost. By adding phosphorus pentoxide, the melting temperature of the glass raw materials can be effectively reduced. Furthermore, when used in combination with other raw material components, the stability and visible light transmittance of the glass are improved, resulting in phosphate optical glass with a refractive index of 1.94-1.96 and an Abbe number of 23-24. It exhibits low relative partial dispersion, excellent transmittance, chemical stability, and mechanical properties, making it suitable for optical glass applications with high requirements for optical lenses. Moreover, the use of raw material mixing equipment in the glass preparation process enables efficient mixing and facilitates mass production.

[0106] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are merely preferred examples and are not intended to limit the invention. Various changes and modifications can be made to the invention without departing from its spirit and scope, and all such changes and modifications fall within the scope of the present invention as claimed. The scope of protection of the present invention is defined by the appended claims and their equivalents.

Claims

1. A phosphate optical glass, characterized in that, It is composed of the following raw materials in the indicated weight ratios: 35-45 parts aluminum metaphosphate, 18-23 parts barium metaphosphate, 8-22 parts phosphorus pentoxide, 3-7 parts niobium pentoxide, 0.5-1.5 parts antimony trioxide, 5-15 parts tungsten oxide, 6-10 parts titanium oxide, 4-10 parts sodium oxide, and 5-9 parts zirconium dioxide. The aluminum metaphosphate is aluminum metaphosphate without lanthanum and yttrium doping; The refractive index of the phosphate optical glass ranges from 1.94 to 1.96, and the Abbe number ranges from 23 to 24.

2. A process for preparing phosphate optical glass, used to prepare the phosphate optical glass according to claim 1, characterized in that, Includes the following steps: S1. Weigh the raw materials aluminum metaphosphate, barium metaphosphate, phosphorus pentoxide, niobium pentoxide, antimony trioxide, tungsten oxide, titanium oxide, sodium oxide and zirconium dioxide according to the proportion using a weighing device, and set the weighed raw materials aside. S2. The prepared raw materials, namely aluminum metaphosphate, barium metaphosphate, phosphorus pentoxide, niobium pentoxide, antimony trioxide, tungsten oxide, titanium oxide, sodium oxide and zirconium dioxide, are measured and mixed using a raw material mixing device to ensure that the raw materials are mixed evenly. S3. Place the evenly mixed raw materials into a quartz ceramic crucible and perform initial melting. Raise the temperature to a high temperature for melting, stirring and homogenizing during the process. After stirring, raise the temperature to 1360-1420℃ and keep it at that temperature for 5-10 hours to clarify the material and allow the bubbles to rise fully. After the raw materials have melted into glass liquid, cool them down. S4. After melting is complete, pour or strain the molten glass into a preheated mold to form it, and then place the formed glass in an annealing furnace for annealing.

3. The preparation process of phosphate optical glass according to claim 2, characterized in that: In step S3, the initial melting temperature in the quartz ceramic crucible is between 1150℃ and 1250℃.

4. The preparation process of phosphate optical glass according to claim 2, characterized in that: The stirring time in step S3 is controlled at 2.5-6 hours.

5. The preparation process of phosphate optical glass according to claim 2, characterized in that: The temperature of the cooling process in step S3 is reduced to 1050-1200℃.

Citation Information

Patent Citations

  • A phosphate optical glass, its preparation method, optical elements, and filters.

    CN108675631B

  • Optical glass, preform and optical element

    CN102712523A

  • Asynchronous stirring tank

    CN104549029A

  • Phosphate optical glass and preparation method thereof

    CN116239301A