Preparation method and application of titanium carbide supported bismuth oxybromide nanoparticle material for photocatalytic degradation of roxarsone in water

By preparing titanium carbide-supported bismuth oxybromide nanoparticles N-BiOBr/Ti₃C₂, the problems of low visible light utilization and rapid charge recombination in photocatalytic systems were solved, achieving efficient degradation of roxarsone in water and improving the removal rate and degradation efficiency of organic arsenic.

CN118384904BActive Publication Date: 2026-11-20NORTHEAST FORESTRY UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410505452.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-25
Publication Date
2026-11-20
Estimated Expiration
2044-04-25

AI Technical Summary

Technical Problem

Existing photocatalytic systems suffer from low visible light utilization, rapid charge recombination, and poor electron and hole migration capabilities, making it difficult to efficiently degrade roxarsone in water.

Method used

By using titanium carbide-supported bismuth oxybromide nanoparticles N-BiOBr/Ti₃C₂, and combining the semiconductor materials N-BiOBr and Ti₃C₂, the visible light utilization and electron-hole migration ability of the photocatalyst are improved, thereby enhancing its oxidation ability of organic arsenic.

Benefits of technology

The system achieved a high removal rate of over 70% for organic arsenic under ambient temperature conditions, shortening the reaction time, reducing costs, and avoiding secondary pollution from inorganic arsenic compounds.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118384904B_ABST
    Figure CN118384904B_ABST
Patent Text Reader

Abstract

The application relates to a preparation method and application of a titanium carbide loaded bismuth oxybromide nanoparticle material for photocatalytic degradation of roxarsone in water, and aims to solve the problems of low visible light utilization rate, fast charge recombination speed, poor migration ability of photo-generated electrons and holes and the like of a catalyst in an existing photocatalytic system. The preparation method comprises the following steps: I, ultrasonic mixing of C2H5OH and Bi(NO3)3.5H2O, dropwise addition of a KBr solution under stirring to generate a BiOBr material; II, dissolving the BiOBr material and phloroglucinol in deionized water, and hydrothermal reaction to obtain an N-BiOBr material; III, mixing and dispersing the N-BiOBr material and Ti3C2 in an organic solvent, stirring reaction, and ultrasonic treatment. The N-BiOBr / Ti3C2 catalyst prepared in the application can realize a removal rate of organic arsenic of more than 70% in 3h under normal temperature conditions by optimizing the preparation conditions and reaction conditions of the catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of wastewater treatment using photocatalytic semiconductor materials, specifically relating to a method for preparing a titanium carbide-supported bismuth oxybromine nanoparticle (N-BiOBr / Ti3C2) catalyst and its application in the efficient degradation of roxarsone in water. Background Technology

[0002] Roxarsone is used as an organic arsenic feed additive to promote animal growth and treat coccidiosis. However, most of the roxarsone added to the feed is not absorbed by the animals and is ultimately retained in their feces after digestion. Because roxarsone is highly water-soluble, it easily migrates from animal feces to the surrounding aquatic environment. Currently reported organic arsenic removal technologies mainly include biological methods, adsorption methods, and advanced oxidation processes. Photocatalysis, as an advanced oxidation process, has the advantages of producing a large amount of highly oxidizing active substances and no secondary pollution. However, if the oxidized inorganic arsenic compounds are not treated properly in a timely manner, the highly toxic inorganic arsenic compounds can cause serious environmental pollution. Therefore, the "oxidation + adsorption" technology for treating organic arsenic in water has received widespread attention. The incorporation of noble metals into photocatalysts as auxiliary catalysts has been widely used, but their high price and scarcity limit their practical application. Therefore, this invention designs a noble metal-free catalyst, N-BiOBr / Ti3C2. The modified catalyst has advantages such as excellent conductivity, large specific surface area, and multiple active sites. Summary of the Invention

[0003] The purpose of this invention is to solve the problems of low visible light utilization rate, fast charge recombination rate, and poor electron and hole migration ability of existing photocatalytic systems, so as to provide a method for preparing titanium carbide-supported bismuth oxybromine nanoparticles for photocatalytic degradation of roxarsone in water and to improve the application of photocatalytic degradation of organic arsenic in water.

[0004] The preparation method of titanium carbide-supported bismuth oxybromide nanoparticles for photocatalytic degradation of roxarsone in water according to the present invention is carried out according to the following steps:

[0005] 1. Dissolve KBr in deionized water and heat to 80-90℃ to obtain KBr solution; mix C2H5OH and Bi(NO3)3·5H2O ultrasonically until Bi(NO3)3·5H2O dissolves to form a suspension, and add KBr solution dropwise under stirring to react and generate BiOBr material;

[0006] 2. Dissolve BiOBr material and phloroglucinol (C6H6O3) in deionized water and stir the reaction at 50-70℃. Then, perform hydrothermal treatment at 180-240℃ for 10-15 hours. After washing and drying, the reaction product is used to obtain N-BiOBr material.

[0007] III. N-BiOBr material and Ti3C2 were mixed and dispersed in an organic solvent, stirred and reacted, and then ultrasonically treated. After washing and drying, titanium carbide-supported bismuth oxybromide nanoparticles N-BiOBr / Ti3C2 were obtained for photocatalytic degradation of roxarsone in water.

[0008] In step three, the mass ratio of N-BiOBr to Ti3C2 is 1:(5-20).

[0009] The application of the titanium carbide-supported bismuth oxybromide nanoparticle material for photocatalytic degradation of roxarsone in water in this invention involves placing the titanium carbide-supported bismuth oxybromide nanoparticle material N-BiOBr / Ti3C2 in water containing roxarsone, and then catalytically degrading the roxarsone in the water under visible light irradiation.

[0010] This invention provides a catalyst for the photocatalytic degradation of roxarsone: a supported N-BiOBr / Ti3C2 composite catalyst is obtained by combining the semiconductor material N-BiOBr with Ti3C2 in a solvent phase. N-BiOBr consists of BiOBr nanoparticles, and Ti3C2 is an MXenes material. Calculations using Mulliken electronegativity theory show that N-BiOBr, as a semiconductor material, has a more positive valence band ratio than the standard redox potentials of ·OH / OH-, H2O2, and O3, thus exhibiting stronger oxidizing properties and enhancing the visible light-driven oxidation of organic arsenic to inorganic arsenic. Due to the large specific surface area and more adsorption active sites of Ti3C2, it has a higher adsorption efficiency for arsenic, thereby removing arsenic from water.

[0011] The N-BiOBr / Ti3C2 catalyst prepared by this invention can achieve an organic arsenic removal rate of over 70% in 3 hours at room temperature by optimizing the catalyst preparation and reaction conditions.

[0012] This invention provides a novel approach for removing organic arsenic from water. It involves oxidizing organic arsenic into inorganic arsenic compounds, followed by adsorption to remove these compounds from the water promptly, thus avoiding secondary pollution. Furthermore, by modifying the surface of Ti3C2 with N-BiOBr, a highly efficient N-BiOBr / Ti3C2 oxidation adsorption compound is obtained. This preparation process is simple, has high catalytic efficiency, shortens the arsenic removal time from water, and operates under mild reaction conditions, eliminating the need for pure oxygen or organic solvents, thereby reducing costs. Attached Figure Description

[0013] Figure 1 Here is a scanning electron microscope image of Ti3C2 in the example;

[0014] Figure 2The image shows a scanning electron microscope (SEM) image of the 5% N-BiOBr / Ti3C2 material obtained in the examples.

[0015] Figure 3 The image shows a scanning electron microscope (SEM) image of the 10% N-BiOBr / Ti3C2 material obtained in the examples.

[0016] Figure 4 The image shows a scanning electron microscope (SEM) image of the 20% N-BiOBr / Ti3C2 material obtained in the examples.

[0017] Figure 5 The image shows the XRD pattern of the N-BiOBr / Ti3C2 composite material obtained in the examples. Detailed Implementation

[0018] Specific Implementation Method 1: The preparation method of titanium carbide-supported bismuth oxybromide nanoparticles for photocatalytic degradation of roxarsone in water in this implementation method is carried out according to the following steps:

[0019] 1. Dissolve KBr in deionized water and heat to 80-90℃ to obtain KBr solution; mix C2H5OH and Bi(NO3)3·5H2O ultrasonically until Bi(NO3)3·5H2O dissolves to form a suspension, and add KBr solution dropwise under stirring to react and generate BiOBr material;

[0020] 2. Dissolve BiOBr material and phloroglucinol (C6H6O3) in deionized water and stir the reaction at 50-70℃. Then, perform hydrothermal treatment at 180-240℃ for 10-15 hours. After washing and drying, the reaction product is used to obtain N-BiOBr material.

[0021] 3. N-BiOBr material and Ti3C2 material are mixed and dispersed in an organic solvent, wherein the Ti3C2 material is an accordion-shaped multilayer Ti3C2 powder. After stirring and reacting, the mixture is ultrasonically treated, washed and dried to obtain titanium carbide-supported bismuth oxybromide nanoparticle material N-BiOBr / Ti3C2 for photocatalytic degradation of roxarsone in water.

[0022] In step three, the mass ratio of N-BiOBr to Ti3C2 is 1:(5-20).

[0023] The preparation method of N-BiOBr / Ti3C2 for the photocatalytic degradation of roxarsone in water in this embodiment is simple and safe. In step three of this embodiment, the Ti3C2 used is an accordion-shaped multilayer Ti3C2 powder. The accordion-shaped multilayer Ti3C2 material has a higher specific surface area, improving the adsorption and catalytic performance of the catalyst; it also gives the catalyst good flexibility, enabling it to withstand large deformations, thus making the catalyst plastic; and it improves the catalyst's electrical conductivity and high chemical reactivity. The generated BiOBr nanoparticles can uniformly adhere to the surface of the accordion-shaped Ti3C2, improving photocatalytic efficiency while having minimal impact on Ti3C2 adsorption.

[0024] BiOBr, as a photocatalytic material, possesses a suitable band gap, an open layered structure, high oxidation capacity, an indirect transition mode, high visible light response, and excellent stability. In this embodiment, BiOBr is synthesized into spherical form using a hot solvent method. Due to the small interlayer spacing of Ti3C2, BiOBr cannot adhere to the surface; therefore, the BiOBr material is prepared as nanoparticles to attach to the Ti3C2 surface. These treated BiOBr nanoparticles are denoted as N-BiOBr.

[0025] Specific Implementation Method Two: This implementation method differs from Specific Implementation Method One in that the molar ratio of KBr and Bi(NO3)3·5H2O in step one is 1:1.

[0026] Specific Implementation Method 3: This implementation method differs from Specific Implementation Method 1 or 2 in that the reaction is stirred at 60°C for 1.5 to 2.5 hours in step 2.

[0027] Specific Implementation Method Four: This implementation method differs from Specific Implementation Methods One to Three in that step two involves hydrothermal treatment at 200°C for 11 to 13 hours.

[0028] Specific Implementation Method 5: This implementation method differs from Specific Implementation Methods 1 to 4 in that the mass ratio of N-BiOBr material to Ti3C2 material in step 3 is 1:10.

[0029] Specific Implementation Method Six: This implementation method differs from Specific Implementation Methods One to Five in that, after stirring and reacting for 10 to 14 hours in step three, the mixture is ultrasonically treated for 1 to 2 hours.

[0030] Specific Implementation Method Seven: This implementation method differs from Specific Implementation Methods One to Six in that the organic solvent mentioned in step three is DMSO.

[0031] Specific Implementation Method 8: The application of titanium carbide-supported bismuth oxybromide nanoparticles for photocatalytic degradation of roxarsone in water in this implementation method involves placing titanium carbide-supported bismuth oxybromide nanoparticles N-BiOBr / Ti3C2 in water containing roxarsone, and then catalytically degrading roxarsone in the water under visible light irradiation.

[0032] Specific Implementation Method Nine: This implementation method differs from Specific Implementation Method Eight in that the titanium carbide-supported bismuth oxybromide nanoparticle material N-BiOBr / Ti3C2 is placed in water containing roxarsone, and the pH of the system is adjusted to 7-8.

[0033] Specific Implementation Method 10: This implementation method differs from Specific Implementation Methods 8 or 9 in that the visible light used is a xenon lamp or an ultraviolet lamp.

[0034] Example: The preparation method of the titanium carbide-supported bismuth oxybromide nanoparticle material for photocatalytic degradation of roxarsone in water in this example is carried out according to the following steps:

[0035] 1. Dissolve 0.67g of KBr (potassium bromide) in 75mL of deionized water at room temperature and heat to 90℃ to obtain KBr solution; mix 100mL of C2H5OH and 2.43g of Bi(NO3)3·5H2O by ultrasonication until Bi(NO3)3·5H2O dissolves to form a suspension; add KBr solution dropwise under stirring and react for 30min to generate BiOBr material (pale yellow precipitate);

[0036] 2. Dissolve 1.07g BiOBr and 0.27g phloroglucinol (C6H6O3) in 40ml of distilled water, stir and react at 60℃ for 2h, then hydrothermally treat at 200℃ for 12h, wash the reaction product with water and ethanol three times respectively, and dry at 60℃ for 6h to obtain N-BiOBr material.

[0037] 3. Different masses of N-BiOBr material and accordion-shaped multilayer Ti3C2 powder were mixed and dispersed in 40 ml of DMSO, stirred and reacted at room temperature for 12 h, then sonicated for 1 h, washed three times with water and ethanol respectively, and dried at 60 °C for 8 h to obtain N-BiOBr / Ti3C2 material for photocatalytic degradation of roxarsone in water.

[0038] In this embodiment, N-BiOBr / Ti3C2 composite materials with N-BiOBr loadings of 5 wt%, 10 wt%, and 20 wt% were prepared. When the N-BiOBr loading was 5 wt%, the mass ratio of N-BiOBr material to Ti3C2 in step three was 1:20. When the N-BiOBr loading was 10 wt%, the mass ratio of N-BiOBr material to Ti3C2 in step three was 1:10. When the N-BiOBr loading was 20 wt%, the mass ratio of N-BiOBr material to Ti3C2 in step three was 1:5.

[0039] The XRD pattern of N-BiOBr / Ti3C2 obtained in this embodiment is as follows: Figure 5 As shown, Figure 5 The material exhibits characteristic peaks of both N-BiOBr and Ti3C2. N-BiOBr modification of Ti3C2 does not alter the structure of Ti3C2, as shown in the following example. Figures 2-4 The image shows a scanning electron microscope (SEM) image of the prepared N-BiOBr / Ti3C2 composite material. The surface is uneven, which provides more active sites.

[0040] Application Example 1: In this example, a 300W light source was used to filter out wavelengths with λ < 420nm to simulate a visible light source. 0.05g of pure titanium carbide and 50ml of roxarsone aqueous solution with a concentration of 2mg / L and pH = 7 were mixed in a three-necked flask with a cooling water circulation device. The light source was turned on and the mixture was magnetically stirred for 3 hours. The organic arsenic in the water was removed by photocatalytic reaction under visible light irradiation.

[0041] In this embodiment, the catalyst in the reaction solution was removed by centrifugation, and then the reaction solution was filtered through an organic filter membrane (0.22 μm). The organic arsenic removal rates were measured by UV spectrophotometer at various reaction time intervals of 30 min, 60 min, 90 min, 120 min, and 180 min, respectively, and were 30.5%, 36.1%, 38.8%, 40.1%, and 44.5%.

[0042] Application Example 2: In this example, a 300W light source was used. The wavelength range of λ < 420nm was filtered out by a filter device to simulate a visible light source. 0.05g of supported 5wt% N-BiOBr / Ti3C2 (i.e., N-BiOBr accounts for 5% of the mass of N-BiOBr / Ti3C2 material) and 50ml of roxarsone aqueous solution were mixed in a three-necked flask with a cooling water circulation device. The light source was turned on and the mixture was magnetically stirred for 3 hours. The organic arsenic in the water was removed by photocatalytic reaction under visible light irradiation.

[0043] In this embodiment, the catalyst in the reaction solution was removed by centrifugation, and then the reaction solution was filtered through an organic filter membrane (0.22 μm). The organic arsenic removal rates were measured by UV spectrophotometer at various reaction time intervals of 30 min, 60 min, 90 min, 120 min, and 180 min, respectively, and were 68.3%, 74.5%, 75.8%, 76.4%, and 75.8%, respectively.

[0044] Application Example 3: In this example, a 300W light source was used. A filter was used to remove wavelengths < 420nm to simulate a visible light source. 0.05g of supported 10wt% N-BiOBr / Ti3C2 (i.e., N-BiOBr accounts for 10% of the mass of the N-BiOBr / Ti3C2 material) and 50ml of roxarsone aqueous solution were mixed in a three-necked flask equipped with a cooling water circulation device. The light source was turned on, and the mixture was magnetically stirred for 3 hours. The photocatalytic reaction under visible light irradiation removed organic arsenic from the water. Experimental results showed that 10wt% N-BiOBr / Ti3C2 exhibited the best photocatalytic effect.

[0045] In this embodiment, the catalyst in the reaction solution was removed by centrifugation, and then the reaction solution was filtered through an organic filter membrane (0.22 μm). The organic arsenic removal rates were measured by UV spectrophotometer at various reaction time intervals of 30 min, 60 min, 90 min, 120 min, and 180 min, respectively, and were 36.7%, 50.0%, 58.9%, 65.6%, and 73.3%.

[0046] Application Example 4: In this example, a 300W light source was used to filter out wavelengths with λ < 420nm to simulate a visible light source. 0.05g of supported 20wt% N-BiOBr / Ti3C2 (i.e., N-BiOBr accounts for 20% of the mass of N-BiOBr / Ti3C2 material) and 50ml of roxarsone aqueous solution were mixed in a three-necked flask with a cooling water circulation device. The light source was turned on, and the mixture was magnetically stirred for 3 hours. The organic arsenic in the water was removed by photocatalytic reaction under visible light irradiation.

[0047] In this embodiment, the catalyst in the reaction solution was removed by centrifugation, and then the reaction solution was filtered through an organic filter membrane (0.22 μm). The organic arsenic removal rates were measured by UV spectrophotometer at various reaction time intervals of 30 min, 60 min, 90 min, 120 min, and 180 min, respectively, and were 22.8%, 28.2%, 31.3%, 34.7%, and 38.2%.

[0048] Experiments show that a loading of 10 wt% N-BiOBr / Ti3C2 has the best effect on the removal of organic arsenic. When the loading of N-BiOBr is too low, the catalytic efficiency of the catalyst is too low and the catalytic time is too long. When the loading of N-BiOBr is too high, the activity of the catalyst will decrease sharply, resulting in a decrease in catalytic efficiency.

Claims

1. A method for preparing titanium carbide-supported bismuth oxybromide nanoparticles for photocatalytic degradation of roxarsone in water, characterized in that... The preparation method is carried out according to the following steps:

1. Dissolve KBr in deionized water and heat to 80-90℃ to obtain a KBr solution; mix C2H5OH and Bi(NO3)3·5H2O ultrasonically until Bi(NO3)3·5H2O dissolves to form a suspension; add KBr solution dropwise under stirring to react and generate BiOBr material; the molar ratio of KBr to Bi(NO3)3·5H2O is 1:

1.

2. Dissolve BiOBr material and phloroglucinol in deionized water, stir and react at 50-70℃, then hydrothermally treat at 180-240℃ for 10-15 hours. After washing and drying, N-BiOBr material is obtained. III. N-BiOBr material and Ti3C2 were mixed and dispersed in an organic solvent, stirred and reacted, and then ultrasonically treated. After washing and drying, titanium carbide-supported bismuth oxybromide nanoparticles N-BiOBr / Ti3C2 were obtained for photocatalytic degradation of roxarsone in water. In step three, the mass ratio of N-BiOBr to Ti3C2 is 1:

10.

2. The method for preparing titanium carbide-supported bismuth oxybromide nanoparticles for photocatalytic degradation of roxarsone in water according to claim 1, characterized in that... In step two, the reaction is stirred at 60°C for 1.5–2.5 hours.

3. The method for preparing titanium carbide-supported bismuth oxybromide nanoparticles for photocatalytic degradation of roxarsone in water according to claim 1, characterized in that... In step two, the mixture is hydrothermally treated at 200℃ for 11–13 hours.

4. The method for preparing titanium carbide-supported bismuth oxybromide nanoparticles for photocatalytic degradation of roxarsone in water according to claim 1, characterized in that... After stirring and reacting for 10–14 hours in step three, the mixture is ultrasonically treated for 1–2 hours.

5. The method for preparing titanium carbide-supported bismuth oxybromide nanoparticles for photocatalytic degradation of roxarsone in water according to claim 1, characterized in that... The organic solvent mentioned in step three is DMSO.

6. The application of the titanium carbide-supported bismuth oxybromide nanoparticle material for photocatalytic degradation of roxarsone in water prepared as claimed in claim 1, characterized in that... Titanium carbide-supported bismuth oxybromide nanoparticles N-BiOBr / Ti3C2 were placed in water containing roxarsone, and the roxarsone in the water was catalytically degraded under visible light irradiation.

7. The application of the titanium carbide-supported bismuth oxybromide nanoparticle material for photocatalytic degradation of roxarsone in water according to claim 6, characterized in that... Titanium carbide-supported bismuth oxybromide nanoparticles N-BiOBr / Ti3C2 were placed in water containing roxarsone, and the pH of the system was adjusted to 7-8.

Citation Information

Patent Citations

  • Halogen bismuth oxide / titanium carbide photocatalysis composite material and preparing method thereof

    CN110064424A

  • Bismuth-based photocatalytic MXene membrane material and preparation method thereof

    CN114433226A