Device and method for dynamic control of liquid flux composition for continuous casting
By monitoring and replenishing the composition of liquid protective slag in real time, the problem of performance deterioration caused by compositional changes in liquid protective slag during continuous casting of steel grades was solved, thereby achieving stability of protective slag performance and improvement of billet quality.
Patent Information
- Application Number
- CN202311095878.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-29
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-08-29
AI Technical Summary
During the continuous casting of steel grades, the violent reaction between the liquid protective slag and the crystallizer leads to changes in composition, deteriorates the performance of the protective slag, and causes problems such as cracks, depressions, inclusions and steel leakage in the cast billet, which cannot be effectively solved by existing technologies.
A device and method for dynamic control of the composition of external liquid protective slag in continuous casting are designed. The composition changes of the liquid protective slag are monitored in real time through a composition monitoring system. A composite system is used to melt the solid powder slag into liquid in advance and replenish the consumed components in real time according to the calculation results to maintain the stability of the composition ratio of the protective slag.
It stabilized the viscosity, crystallinity, and heat transfer properties of the protective slag, ensuring the stability of the continuous casting process, improving the quality of the cast billet, and avoiding compositional fluctuations caused by steel slag reaction.
Smart Images

Figure CN118385496B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of liquid protective slag in continuous casting crystallizers for iron and steel metallurgy. Addressing the issue that some steel grades are prone to violent reactions with the liquid protective slag in the crystallizer during continuous casting, leading to significant changes in the slag composition and consequently deteriorating the slag's performance, resulting in a series of problems such as billet cracks, depressions, inclusions, and even steel leakage, this invention designs a device and method for dynamically controlling the composition of the external liquid protective slag in continuous casting. This maintains the "dynamic stability" of each component of the protective slag, allowing it to play its proper role and further improving billet quality while stabilizing the continuous casting production process. Background Technology
[0002] Liquid protective slag in continuous casting molds is a molten liquid slag layer added and spread onto the surface of the molten steel in the mold. Its main function is to stabilize the continuous casting process and improve the surface quality of the cast billet. Unlike the pre-melted solid powder slag widely used in current continuous casting production, liquid protective slag is melted into a liquid state by external melting equipment and then added to the surface of the molten steel in the mold, replacing the solid powder slag. Compared to solid powder slag, using liquid protective slag can achieve a lower meniscus, a smaller slag ring, and better lubrication. Furthermore, the external melting equipment and liquid slag transfer device can reasonably control the temperature and thickness of the added liquid protective slag layer, thus achieving good adaptability to casting different steel grades. However, in the production of high-alumina steel with intense steel-slag interface reactions, the aluminum [Al] in the steel reacts with (SiO2) in the slag to form Al2O3, which enters the slag, causing an increase in the basicity of the protective slag. This deteriorates the viscosity, melting temperature, crystallization, and heat transfer properties, leading to defects such as depressions and cracks in the cast billet, and even causing leaks. Meanwhile, to obtain favorable physicochemical properties of the protective slag, conventional protective slags require the addition of certain amounts of fluxes such as Ca2F, Na2O, and K2O to lower their melting point and viscosity. These compounds pose significant risks to the environment and human health. Previous solutions to this problem have focused on reducing the SiO2 content in the slag to decrease steel slag reactivity, but this approach has not been effective, resulting in persistent billet quality defects and hindering continuous casting. This project addresses this issue by designing a device and method for dynamically controlling the composition of externally added liquid protective slag in continuous casting. This aims to resolve the compositional changes in the liquid protective slag caused by steel slag reaction and slag consumption, maintaining stable physicochemical properties and ensuring the smooth operation of the continuous casting process while further improving billet quality.
[0003] Chinese invention patent application number CN201210129762.2 discloses a continuous casting mold flux addition device and its operation method, including a screw conveyor (1); a tank (2); a heating device (3); a traveling trolley (4); a control cabinet (5); a swing arm spreading device (6); a connecting rod compensation device (7); and a stirring device (8). The process involves manually disassembling the mold flux and pouring it into the tank (2). The control cabinet (5) controls the swing arm spreading device (6) to move back and forth, while the mold flux is spread onto the molten steel surface via the screw conveyor (1). This solution solves the problems of low work efficiency and cost waste in manual mold flux addition, achieving automation of the mold flux addition process. However, the shortcomings of this solution are that the mold flux still requires manual disassembly and assembly, resulting in low automation; the amount of slag added is difficult to control precisely; the addition of the mold flux in solid form still causes fluctuations in the molten steel temperature, easily affecting the stable operation of the continuous casting process; and it cannot solve the problem of the slag reaction causing deterioration of the mold flux performance.
[0004] The utility model patent with application number CN202221623193.2 discloses an automatic feeder for protective slag, including a workbench (1); a conveying device (5); a filtering device (14); a connecting pipe (13); a conveying cylinder (2); and a vibration device (18). In this scheme, the protective slag is added to the surface of the molten steel in the crystallizer after being filtered by vibration. While filtering the protective slag, it can avoid the accumulation of protective slag and improve the continuous casting production efficiency. The shortcomings of this scheme are that the device needs to be arranged directly above the crystallizer, and the process of screening and filtering the protective slag will generate a large amount of vibration, which poses a significant safety hazard; the protective slag is still added in solid form, which will cause fluctuations in the temperature of the molten steel and easily affect the stable operation of the continuous casting process; and it cannot solve the problem of the steel slag reaction causing the performance of the protective slag to deteriorate. Summary of the Invention
[0005] The purpose of this invention is to provide a device and method for dynamic control of the composition of external liquid protective slag in continuous casting. Through various composite system devices, solid powdered slag is pre-melted into a liquid state for storage. A composition monitoring system monitors the changes in the composition of the liquid protective slag in real time. A calculation method that maintains the ratio of the changed protective slag components to the original components is used to continuously calculate the amount of a certain liquid slag component that needs to be replenished at different times. The "consumed component" is replenished in real time to the liquid protective slag on the surface of the molten steel in the crystallizer to maintain the "dynamic stability" of the protective slag composition. This maintains the stability of the protective slag's viscosity, crystallinity, and heat transfer properties, ensuring the stable and smooth operation of the continuous casting process and improving the quality of the cast billet.
[0006] To achieve the above objectives, the present invention provides the following technical solution: a device and method for dynamic control of the composition of externally added liquid protective slag in continuous casting, comprising a control terminal, a crystallizer external to the control terminal, a plurality of composition monitoring systems and a plurality of liquid slag inlet ports inserted on the crystallizer, an immersion port inserted on the crystallizer, a composite system ⑤ on the upper side of the crystallizer, the composite system ⑤ being connected to the liquid slag inlet ports via a liquid slag conveying system, a plurality of composite systems ① on the upper side of the composite system ⑤, and composite systems ②, ③ and ④ sequentially arranged on the lower side of the composite systems ①, the composite system ⑤ being connected to the composite system ④.
[0007] Preferably, the composite system ① includes a hopper, which is positioned above the mixing device. An automatic feeding system is installed at the bottom of the hopper, and an automatic weighing system is installed below the automatic feeding system. The automatic weighing system transmits weighing data information to the control terminal.
[0008] Furthermore, the number of hoppers is determined by the composition of the protective slag, and the number can be set to 3-6. Each hopper can work independently without affecting each other, so as to realize the separate storage of each component base material.
[0009] The hopper is equipped with an automatic feeding system to achieve automated control of the feeding process;
[0010] An automatic weighing system is installed below the hopper to accurately weigh the amount of protective slag component base material used.
[0011] The hopper, automatic feeding system, and automatic weighing system constitute an independent composite system①, which work together in coordination to complete the automatic feeding and weighing process of the base material components. The weighing data information will be transmitted to the control terminal in real time.
[0012] Preferably, the composite system ② includes a component conveying device, which is located below the automatic weighing system. A dustproof cover is installed on the lower side of the component conveying device, and a component transport pipe is installed between the dustproof cover and the component conveying device.
[0013] Furthermore, a component conveying device is provided below the automatic weighing system to control the conveying process of the component base material;
[0014] The component transport pipeline is connected to the component conveying device and is used to transport the protective slag base material components;
[0015] The dust cover is connected to the component transport pipeline to reduce the dispersion of component base materials and reduce dust.
[0016] The component conveying device, component transport pipeline and dustproof cover constitute an independent composite system ②, which coordinates and cooperates to complete the base material component conveying process, and the conveying process information will be transmitted to the control terminal in real time.
[0017] Preferably, the composite system ③ includes a component melting system, which is disposed on the lower side of the dustproof cover. The feed end of the component melting system is connected to the dustproof cover. A support column is installed outside the component melting system, and a motor rotation system is installed outside the component melting system. The motor rotation system is connected to the support column.
[0018] Furthermore, the supporting column is used to support the component melting system;
[0019] The component melting system is used to heat and melt the protective slag base material components to a liquid state and raise the temperature to a set temperature;
[0020] The number of component melting systems is determined by the composition of the protective slag, and the number can be set to 3-6. Each component melting system can work independently without affecting each other, so as to achieve separate melting of each component.
[0021] The component melting system is equipped with a motor rotation system to control the process of pouring qualified component liquid slag into the component melting system;
[0022] The supporting column, component melting system and motor rotation system constitute an independent composite system③, which coordinates and cooperates to complete the feeding, slag melting and slag dumping processes, and the slag melting information will be transmitted to the control terminal in real time.
[0023] Preferably, the composite system ④ includes a liquid slag component storage system, which is located outside the component melting system. A flow control system is installed on the liquid slag component storage system, and the flow control system is connected to the composite system ⑤ through the liquid slag component conveying system. A temperature control system is installed inside the liquid slag component storage system.
[0024] Furthermore, the liquid slag component storage system is used to store qualified liquid slag poured out by the component melting system;
[0025] The liquid residue component storage system is equipped with a flow control system for precisely controlling the outflow of component liquid residue;
[0026] The liquid residue component storage system is equipped with a temperature control system for monitoring temperature changes in the stored liquid residue.
[0027] The liquid residue component storage system, flow control system and temperature control system constitute a composite system④, which coordinates and cooperates to realize the storage, flow control and temperature control process of qualified component liquid residue. When necessary, the temperature of the stored liquid residue can be adjusted, and the storage information will be transmitted to the control terminal in real time.
[0028] The liquid sludge component conveying system is connected to the liquid sludge component storage system and is used to transport the liquid sludge flowing out of the liquid sludge component storage system;
[0029] The liquid slag components conveyed by the liquid slag component conveying system enter the mixing device through the inlet of the mixing device for thorough mixing.
[0030] Preferably, the composite system ⑤ mixing device is located below the liquid slag component storage system. The mixing device is provided with a mixing inlet, which is connected to the liquid slag component conveying system. The mixing device is equipped with a mixing parameter setting terminal, and a mixing outlet is installed on the lower side of the mixing device, which is connected to the liquid slag conveying system.
[0031] Furthermore, the mixing device is controlled by the mixing parameter setting terminal, and the fully mixed liquid residue flows out through the outlet of the mixing device.
[0032] The mixing device inlet, mixing device, mixing parameter setting terminal and mixing device outlet constitute a composite system⑤, which coordinates and cooperates to complete the full mixing process of component liquid slag, and the mixing process information will be transmitted to the control terminal in real time.
[0033] The outlet of the mixing device is connected to the liquid-sludge conveying system;
[0034] The liquid slag conveying system is connected to the liquid slag inlet. The mixed liquid slag is transported through the liquid slag conveying system and the liquid slag inlet to the liquid slag layer on the surface of the molten steel in the crystallizer to complete the slag addition process.
[0035] The liquid slag inlet is symmetrically arranged, with one in each symmetrical position, which can achieve rapid mixing of the newly added liquid slag with the liquid slag on the surface of the molten steel in the crystallizer.
[0036] The component monitoring system is installed in the liquid slag layer of the crystallizer, with one system on each side symmetrically. It is used to monitor the changes in the composition and temperature of the protective slag in real time, and the collected data will be transmitted to the control terminal in real time.
[0037] Preferably, it includes the following steps:
[0038] 1) The control terminal will receive various types of information collected from composite system ①, composite system ②, composite system ③, composite system ④, and composite system ⑤ in real time;
[0039] 2) The control terminal will aggregate various information collected in real time from each composite system and calculate the amount of a certain component of the liquid slag to be added at that time.
[0040] 3) The method for dynamic control of the composition of external liquid protective slag in continuous casting obtains the amount of a certain liquid slag component to be added at different times by continuously calculating the changes in the content of each component of the protective slag at different times.
[0041] The method for dynamically controlling the composition of external liquid protective slag in continuous casting, which replenishes the "consumed components" of the liquid slag, is based on the principle of maintaining the proportion of each component before and after the reaction of the liquid protective slag.
[0042] 4) The control terminal will transmit the calculation results to composite system ①, composite system ②, composite system ③, composite system ④, and composite system ⑤ in real time;
[0043] 5) The composite systems ①, ②, ③, ④, and ⑤ will receive instructions and automatically control each system component to complete the specified operation;
[0044] 6) The aforementioned composite systems ①, ②, ③, ④, and ⑤ will feed back the instruction execution information to the control terminal in real time;
[0045] 7) The composite system ①, composite system ②, composite system ③, composite system ④, and composite system ⑤ are closely coordinated with the control terminal to replenish the required liquid slag components to the liquid slag layer on the surface of the liquid steel in the crystallizer in real time, so as to maintain the "dynamic stability" of the protective slag components.
[0046] 8) Maintain the stability of the protective slag's viscosity, crystallization, and heat transfer properties to ensure the smooth and stable operation of the continuous casting process;
[0047] Furthermore, the method for dynamic control of the composition of the external liquid protective slag in continuous casting can continuously calculate the amount of specific components of the liquid slag to be replenished at different times. Under the command of the control terminal, the "consumed components" generated by the reaction of steel slag or the consumption of protective slag are replenished to the liquid protective slag layer on the surface of the molten steel in the crystallizer in real time to maintain the "dynamic stability" of the protective slag composition, thereby maintaining the stability of the viscosity, crystallinity and other properties of the protective slag, and stabilizing the continuous casting process.
[0048] Preferably, step 3) includes the following steps:
[0049] First, the analytical expression for the change of protective slag consumption over time in the continuous casting process is established as follows:
[0050]
[0051] In the formula: Q 渣-Consumable amount of protective slag, kg; a—Length of the upper section of the crystallizer, mm; b—Width of the upper section of the crystallizer, mm; ξ—Cross-sectional shape velocity coefficient, m·mm·min⁻¹; ρ—Density of liquid protective slag, g·cm⁻³; l max —Effective length of the crystallizer, in meters; — Solidification coefficient of molten steel in the crystallizer, mm·min⁻⁵; f— Vibration frequency of the crystallizer, min⁻¹; η— Viscosity of liquid protective slag, Pa·s; v— Casting speed, m·min⁻¹; c— Length of the lower section of the crystallizer, mm; d— Width of the lower section of the crystallizer, mm; δ— Thickness of the billet shell when the billet exits the crystallizer, mm; L— Casting length of the billet (slab), m; t—Continuous casting time, min;
[0052] Then, the changes in the components in the liquid protective slag were determined;
[0053] Finally, the calculation and analysis of the amount of each component added at different times in the liquid protective slag were performed.
[0054] Preferably, the determination of the changes in each component in the liquid protective slag step includes:
[0055] Determination of CaO mass percentage content:
[0056]
[0057] In the formula: —CaO content in the liquid protective slag at time t; —Initial CaO content of the liquid protective slag; Q 渣 -Consumable amount of protective slag, kg; M 总 —Total mass of liquid protective slag added to the crystallizer at the initial moment, kg; t —Continuous casting time, min.
[0058] Determination of SiO2 mass percentage content:
[0059]
[0060] In the formula: —SiO2 content of the liquid protective slag at time t; —Initial SiO2 content of liquid protective slag; β—Mass transfer coefficient, m·s; A—Interfacial area, m2; ρ—Density of liquid protective slag, g·cm-3; n—Dimensionless coefficient, 33-35 for ordinary steel and 42-45 for high-quality steel; V—Volume of fluid, m3; t—Continuous casting time, min.
[0061] Determination of Al2O3 mass percentage content:
[0062]
[0063] In the formula: —Al2O3 content in the liquid protective slag at time t; —Al2O3 content at the initial moment of liquid protective slag; —Initial SiO2 content of liquid protective slag; β—Mass transfer coefficient, m·s; A—Interfacial area, m2; ρ—Density of liquid protective slag, g·cm-3; n—Dimensionless coefficient, 33-35 for ordinary steel, 42-45 for high-quality steel; V—Volume of fluid, m3; t—Continuous casting time, min; Q 渣 -Consumable amount of protective slag, kg; M 总 —Total mass of liquid protective slag added to the crystallizer at the initial moment, kg; t —Continuous casting time, min.
[0064] Preferably, the calculation and analysis of the amount of each component added at different times in the step of liquid protective slag includes:
[0065] Record the components in the initial protective slag respectively The reaction continues until time t;
[0066] Record the components in the protective slag Based on the principle of maintaining the composition of the liquid protective slag unchanged, the following relationship exists in the reaction of the steel slag up to time t:
[0067] p:q:k=(p t +x):(q t +y):k t =(pk t ):(qk t ):(kk t )
[0068] Then at time t, w(CaO) % The amount added is x = pk t -p t ,Right now:
[0069]
[0070] In the formula: x - the amount of w(CaO) to be added to the protective slag from continuous casting to time t. % The simplest proportion of initial CaO in the three components of CaO, SiO2, and Al2O3 in the p-protective slag; —Al2O3 content at the initial moment of liquid protective slag; —Initial SiO2 content of liquid protective slag; β—Mass transfer coefficient, m·s; A—Phase interface area, m2; ρ—Density of liquid protective slag, g·cm-3; n—Dimensionless coefficient, 33-35 for ordinary steel and 42-45 for high-quality steel; V—Volume of fluid, m3; t—Continuous casting time, min; —Initial CaO content of the liquid protective slag; Q 渣-Consumable amount of protective slag, kg; M 总 —Total mass of liquid protective slag added to the crystallizer at the initial moment, kg.
[0071] The amount of SiO2 added at time t is y = qk. t -q t ,Right now:
[0072]
[0073] In the formula: y - the amount of w(SiO2) to be added to the protective slag from continuous casting to time t. % ;q-The simplest proportion of initial SiO2 in the three components of CaO, SiO2, and Al2O3 in the protective slag; —Al2O3 content at the initial moment of liquid protective slag; —Initial SiO2 content of liquid protective slag; Q 渣 -Consumable amount of protective slag, kg; M 总 —Total mass of liquid protective slag added to the crystallizer at the initial moment, kg; t —Continuous casting time, min; β —Mass transfer coefficient, m·s; A —Interfacial area, m2; ρ —Density of liquid protective slag, g·cm-3; n —Dimensionless coefficient, 33-35 for ordinary steel and 42-45 for high-quality steel; V —Volume of fluid, m3; t —Continuous casting time, min.
[0074] Beneficial effects
[0075] This invention provides an apparatus and method for dynamically controlling the composition of externally added liquid protective slag in continuous casting. It offers the following advantages: 1) Solid powder slag is melted into a liquid state by external smelting equipment before being added to the surface of the molten steel in the crystallizer, solving the problem of significant temperature fluctuations in the molten steel caused by the direct addition of solid powder slag in traditional methods, thus enhancing the stability of the continuous casting process. 2) The protective slag is liquid with adjustable temperature, allowing for real-time adjustment according to the casting temperature of different steel grades, making it widely applicable. 3) The slag film formed during continuous casting using liquid protective slag is uniform and relatively thick, providing good heat transfer and lubrication for the cast billet. 4) It can effectively improve surface quality problems such as cracks, depressions, and slag inclusions in the cast billet, potentially further improving the quality of continuously cast billets. 5) By adopting a dynamic control method for the composition of liquid protective slag, the required liquid slag components can be replenished to the liquid protective slag layer on the surface of the molten steel in the crystallizer in real time, thereby maintaining the stability of the liquid slag composition and thus maintaining the stability of the protective slag's basicity, viscosity, melting temperature, crystallization and heat transfer properties. This overcomes the problem of large fluctuations in the composition of protective slag caused by strong steel-slag reaction during the continuous casting process, and can further improve the surface quality of the billet while the continuous casting process proceeds smoothly. Attached Figure Description
[0076] Figure 1This is a schematic diagram of the overall structure for dynamic control of the composition of liquid protective slag in a continuous casting crystallizer according to an embodiment of the present invention.
[0077] In the diagram: 1. Hopper; 2. Automatic feeding system; 3. Automatic weighing system; 4. Component conveying device; 5. Component conveying pipeline; 6. Dustproof cover; 7. Support column; 8. Component melting system; 9. Motor rotation system; 10. Liquid slag component storage system; 11. Flow control system; 12. Temperature control system; 13. Liquid slag component conveying system; 14. Mixing inlet; 15. Mixing device; 16. Mixing parameter setting terminal; 17. Mixing outlet; 18. Liquid slag conveying system; 19. Immersion water inlet; 20. Liquid slag inlet; 21. Component monitoring system; 22. Crystallizer; 23. Control terminal. Detailed Implementation
[0078] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0079] Those skilled in the art should connect all electrical components and their compatible power supplies in this case via wires, and should select appropriate controllers according to actual conditions to meet control requirements. The specific connection and control sequence should refer to the working principle described below, where the electrical components are connected in sequence. The detailed connection methods are well-known in the art. The following mainly introduces the working principle and process, without explaining the electrical control.
[0080] Please see Figure 1 The present invention provides a technical solution:
[0081] Example 1:
[0082] A continuous casting crystallizer liquid protective slag grouping and differentiation device includes a hopper, an automatic feeding system, an automatic weighing system, a component conveying device, a component conveying pipeline, a dustproof cover, a support column, a component melting system, a motor rotation system, a liquid slag component storage system, a flow control system, a temperature control system, a liquid slag component conveying system, a mixing device inlet, a mixing device, a mixing parameter setting terminal, a mixing device outlet, a liquid slag conveying system, an immersion nozzle, a liquid slag inlet, a component monitoring system, a crystallizer, and a control terminal. Its features are:
[0083] The aforementioned hopper is an inverted cone-shaped storage container. Its number is determined by the composition of the protective slag, and 3-6 hoppers can be set up. Each hopper can work independently without affecting each other, realizing the classified storage of each component base material.
[0084] The hopper is equipped with an automatic feeding system, which is equipped with a PLC automatic controller to automatically control the opening and closing of the hopper valve, thereby realizing the automated control of the feeding process.
[0085] An automatic weighing system is installed below the hopper. The automatic weighing system is a precision electronic scale used to accurately weigh the protective slag released from the hopper.
[0086] The hopper, automatic feeding system, and automatic weighing system constitute an independent composite system①, which work together in coordination to complete the automatic feeding and weighing process of the base material components. The weighing data information will be transmitted to the control terminal in real time. The control terminal is an integrated computer used to receive information transmitted by each subsystem and to process and send relevant instructions to control the subsystem to complete the corresponding operations.
[0087] The automatic weighing system is equipped with a component conveying device below it. The component conveying device is an inverted cone-shaped container with a blowing function. The blowing function gives the weighed solid protective slag material initial kinetic energy, which facilitates the conveying of the protective slag component base material.
[0088] The component transport pipeline is connected to the component transport device. The component transport pipeline is a fluidized transport pipeline used to transport protective slag base material.
[0089] The dust cover is connected to the component transport pipeline. The dust cover is a sealed cover with embedded refractory material, used to reduce the dispersion of protective slag component base material and reduce dust.
[0090] The component conveying device, component conveying pipeline and dustproof cover constitute an independent composite system ②, which coordinates and cooperates to complete the base material component conveying process, and the conveying process information will be transmitted to the control terminal in real time;
[0091] The supporting column is a steel beam-column used to support the component melting system;
[0092] The component melting system is equipped with an electromagnetic induction heating device, which is used to heat and melt the protective slag base material components to a liquid state and raise the temperature to a set temperature.
[0093] The number of component melting systems is determined by the composition of the protective slag, and the number can be set to 3-6. Each component melting system can work independently without affecting each other, so as to achieve separate melting of each component.
[0094] The component melting system is equipped with a motor rotation system. The core of the motor rotation system is a rotary motor controlled by a PLC, which is used to control the pouring process of the liquid protective slag after melting.
[0095] The supporting column, component melting system and motor rotation system constitute an independent composite system③, which coordinates and cooperates to complete the feeding, slag melting and slag dumping process, and the slag melting information will be transmitted to the control terminal in real time;
[0096] The liquid slag component storage system is a storage container constructed of refractory material, used to store qualified liquid slag poured out from the component melting system;
[0097] The liquid residue component storage system is equipped with a flow control system, which is a switch that is automatically controlled by a PLC to control the opening and closing of valves, and is used to precisely control the outflow of component liquid residue.
[0098] The liquid residue component storage system is equipped with a temperature control system for monitoring temperature changes in the stored liquid residue.
[0099] The liquid residue component storage system, flow control system and temperature control system constitute a composite system④, which coordinates and cooperates to realize the storage, flow control and temperature control process of qualified component liquid residue. When necessary, the temperature of the stored liquid residue can be adjusted, and the storage information will be transmitted to the control terminal in real time.
[0100] The liquid slag component conveying system (a conveying pipeline constructed of refractory material) is connected to the liquid slag component storage system and is used to transport the liquid slag flowing out of the liquid slag component storage system.
[0101] The liquid slag components conveyed by the liquid slag component conveying system enter the mixing device (a container made of refractory material and equipped with a high-temperature resistant stirring paddle) through the inlet for thorough mixing.
[0102] The mixing device controls the mixing intensity via a mixing parameter setting terminal (control button), and the fully mixed liquid residue flows out through the outlet of the mixing device.
[0103] The mixing device inlet, mixing device, mixing parameter setting terminal and mixing device outlet constitute a composite system⑤, which coordinates and cooperates to complete the full mixing process of component liquid slag, and the mixing process information will be transmitted to the control terminal in real time.
[0104] The outlet of the mixing device is connected to the liquid slag conveying system, which is a circular pipe made of refractory material for conveying liquid protective slag.
[0105] The liquid slag conveying system is connected to the liquid slag inlet. The mixed liquid slag is transported through the liquid slag conveying system and the liquid slag inlet to the liquid slag layer on the surface of the molten steel in the crystallizer to complete the slag addition process.
[0106] The liquid slag inlet (a pipe made of refractory material) is symmetrically arranged, with one on each side, which can enable the newly added liquid slag to be quickly mixed with the liquid slag on the surface of the molten steel in the crystallizer.
[0107] The component monitoring system (detection probe) is set in the liquid slag layer of the crystallizer, with one probe on each side at a symmetrical position. It is used to monitor the changes in the composition and temperature of the protective slag in real time, and the collected data will be transmitted to the control terminal in real time.
[0108] Example 2:
[0109] The method for dynamically controlling the composition of externally added liquid protective slag in continuous casting, as described in claim 1, is characterized in that: the method can continuously calculate the amount of specific components of the liquid slag to be replenished at different times, and replenish the liquid protective slag layer on the surface of the molten steel in the crystallizer in real time under the command of the control terminal, thereby maintaining the "dynamic stability" of the protective slag composition, and thus maintaining the stability of the viscosity, crystallinity and other properties of the protective slag, and stabilizing the continuous casting process. The method includes the following steps:
[0110] The control terminal will receive various types of information collected from composite system ①, composite system ②, composite system ③, composite system ④, and composite system ⑤ in real time;
[0111] The control terminal will aggregate various information collected in real time from each composite system and calculate the amount of a certain component of the liquid slag that needs to be added at that moment.
[0112] The method for dynamic control of the composition of external liquid protective slag in continuous casting obtains the amount of a certain liquid slag component to be added at different times by continuously calculating the changes in the content of each component of the protective slag at different times.
[0113] The method for dynamically controlling the composition of external liquid protective slag in continuous casting is based on the principle of maintaining the proportion of each component in the liquid protective slag before and after the reaction.
[0114] The control terminal will transmit the calculation results to composite system ①, composite system ②, composite system ③, composite system ④, and composite system ⑤ in real time;
[0115] The aforementioned composite systems ①, ②, ③, ④, and ⑤ will receive instructions and automatically control each system component to complete the specified operation;
[0116] The aforementioned composite systems ①, ②, ③, ④, and ⑤ will feed back instruction execution information to the control terminal in real time;
[0117] The aforementioned composite systems ①, ②, ③, ④, and ⑤ work closely with the control terminal to replenish the required liquid slag components to the liquid slag layer on the surface of the molten steel in the crystallizer in real time, thereby maintaining the "dynamic stability" of the protective slag components. This ensures the stability of the protective slag's viscosity, crystallization, and heat transfer properties, guaranteeing the smooth operation of the continuous casting process and improving the quality of the cast billet.
[0118] A method for dynamically controlling the composition of external liquid protective slag in continuous casting was designed, and the specific analysis process is as follows:
[0119] Considering that in addition to the reaction of steel slag, the consumption of protective slag during continuous casting also causes fluctuations in the composition of the protective slag, an analytical expression for the change of protective slag consumption over time during continuous casting is first established as follows:
[0120]
[0121] Where: a—length of the upper section of the crystallizer, mm; b—width of the upper section of the crystallizer, mm; ξ—cross-sectional shape velocity coefficient, m·mm·min⁻¹; ρ—density of the liquid protective slag, g·cm⁻³; l max —Effective length of the crystallizer, in meters; — Solidification coefficient of molten steel in the crystallizer, mm·min⁻⁵; f— Vibration frequency of the crystallizer, min⁻¹; η— Viscosity of liquid protective slag, Pa·s; v— Casting speed, m·min⁻¹; c— Length of the lower section of the crystallizer, mm; d— Width of the lower section of the crystallizer, mm; δ— Thickness of the billet shell when the billet exits the crystallizer, mm; L— Casting length of the billet (slab), m; t—Continuous casting time, min.
[0122] Determination of the changes in the components of liquid protective slag:
[0123] Determination of CaO mass percentage content:
[0124]
[0125] In the formula: —Initial CaO content of liquid protective slag —CaO content in the liquid protective slag at time t, M 总 —Total mass of liquid protective slag added to the crystallizer at the initial moment, kg.
[0126] Determination of SiO2 mass percentage content:
[0127]
[0128] In the formula: —Initial SiO2 content of liquid protective slag; —SiO2 content of liquid protective slag at time t; β—mass transfer coefficient, m·s; A—phase interface area, m2; ρ—density of liquid protective slag, g·cm-3; V—volume of fluid, m3; n—dimensionless coefficient, 33-35 for ordinary steel and 42-45 for high-quality steel.
[0129] Determination of Al2O3 mass percentage content:
[0130]
[0131] In the formula: —Al2O3 content in the liquid protective slag at time t; —Al2O3 content at the initial moment of liquid protective slag.
[0132] Analysis of the calculation of the amount of each component added at different times in liquid protective slag:
[0133] First, record the components in the initial protective slag. Record the composition of the protective slag at time t during the reaction. Based on the principle of maintaining the composition of the liquid protective slag unchanged, the following relationship exists in the reaction of the steel slag up to time t:
[0134] p:q:k=(p t +x):(q t +y):k t =(pk t ):(qk t ):(kk t (1.5)
[0135] Then at time t, w(CaO) % The amount added is x = pk t -p t ,Right now:
[0136]
[0137] The amount of SiO2 added at time t is y = qk. t -q t ,Right now:
[0138]
[0139] Example 3:
[0140] A device and method for dynamic control of the composition of liquid protective slag in a continuous casting crystallizer includes a hopper 1, an automatic feeding system 2 on the hopper 1, and an automatic weighing system 3 below the hopper 1. The weighed component base material is transported to the component melting system 8 for heating and melting via a component conveying device 4, a component conveying pipe 5, and a dustproof cover 6. The liquid components that have been melted to a liquid state and have reached the required temperature are poured into the liquid slag component storage system 10 for separate storage and later use under the action of a motor rotation system. Under the command of the control terminal, the liquid slag component storage system 10, in conjunction with the flow control system 11, adds the qualified liquid slag components through the liquid slag component conveying system 13 to the mixing device inlet 14 for thorough mixing via the mixing device inlet 14. The mixed liquid slag is then transported to the protective slag layer on the surface of the molten steel in the crystallizer via the mixing device outlet 17, the liquid slag conveying system 18, and the liquid slag inlet 20.
[0141] As a further aspect of the present invention: the hopper 1 is equipped with an automatic feeding system 2, and an automatic weighing system 3 is provided below the hopper 1. The three constitute a composite system ①. The automatic feeding system 2 and the automatic weighing system 3 work together to ensure the accuracy of feeding and weighing the amount of solid powder.
[0142] As a further embodiment of the present invention: the component conveying device 4, the component conveying pipeline 5 and the dustproof cover 6 constitute a composite system ②, and the weighed base material components will be conveyed through this system;
[0143] As a further embodiment of the present invention: the supporting column 7, the component melting system 8 and the motor rotation system 9 constitute a composite system ③, which is responsible for heating and melting the protective slag base material components transported to the component melting system 8 to a liquid state and controlling it at a qualified temperature, and then responsible for dumping the component liquid slag.
[0144] As a further embodiment of the present invention: the liquid slag component storage system 10 is equipped with a flow control system 11 and a temperature control system 12, which together constitute a composite system ④. This system is responsible for storing the liquid slag poured out by the component melting system 8 and for the constant temperature control process.
[0145] As a further embodiment of the present invention: the mixing device inlet 14, the mixing device 15, the mixing parameter setting end 16 and the mixing device outlet 17 constitute a composite system ⑤, which is responsible for receiving the component liquid sludge transported by the liquid sludge component storage system 10 and mixing it thoroughly.
[0146] As a further aspect of the present invention: the mixed liquid slag is added to the liquid slag layer on the steel surface of the crystallizer 22 through the liquid slag inlet 20 via the liquid slag conveying system 18;
[0147] As a further aspect of the present invention: two liquid slag inlet ports 20 are provided above the crystallizer 22 to ensure the uniformity of liquid slag addition and improve the mixing efficiency;
[0148] As a further aspect of the present invention: two component detection devices 21 are provided above the crystallizer 22 for accurately monitoring the changes in the composition of the liquid residue;
[0149] As a further aspect of the present invention: 4-6 diversion ports can be provided at the lower end of the liquid slag inlet 20. If necessary, argon gas can be used as the carrier gas to make the added liquid slag uniformly mixed in the liquid slag layer above the molten steel in the crystallizer 22, thereby improving the efficiency of dynamic control of the composition of the liquid protective slag.
[0150] As a further aspect of the present invention: the various composite systems and the control terminal interact and transmit data in real time to complete the entire control process.
[0151] The parameters for the continuous casting slab production process in a steel plant are as follows: the crystallizer length is 1200mm, the molten steel level is 200mm from the top of the crystallizer, and the height of the added liquid protective slag is 40mm; a = 1.22m; b = 0.2m; ξ = 18mm·min⁻¹; l max =1m; K 凝固 =25mm·min-0.5; ρ=2800kg·m-3; f=120min-1; v=0.6m·min-1; c=1.2m; d=0.2m; δ=18mm; L=12m; β=1.78×10-4m·s; A=0.12m2; V=0.0234m3; n=40; The initial composition of the liquid protective slag is w(CaO)=40%; w(SiO2)=50%; w(Al2O3)=10%; The initial mass of the liquid protective slag added to the crystallizer is 26.88kg.
[0152] When the continuous casting process has been underway for 3 minutes, the amount of protective slag consumed is:
[0153]
[0154] The weight of the steel billet produced by continuous casting in 3 minutes is 3.3912t, then the amount of protective slag consumed per ton of steel is Qslag / 3.3912=0.81kg·t-1.
[0155] The mass fraction of CaO remaining after 3 minutes of reaction with steel slag is:
[0156]
[0157] The remaining mass fraction of SiO2 after 3 minutes of reaction with steel slag is:
[0158]
[0159] The remaining mass fraction of Al2O3 after 3 minutes of reaction with steel slag is:
[0160]
[0161] The mass fraction of CaO in the protective slag that should be added after the steel slag has reacted for 3 minutes is:
[0162]
[0163] The volume that should be added in liquid CaO component is:
[0164]
[0165] —The volume of CaO in the liquid slag component to be added at time t; ρ CaO —Density of liquid CaO (ρC) a O = 3.35 g·cm⁻³.
[0166] The mass fraction of SiO2 in the protective slag that should be supplemented is:
[0167]
[0168] The volume that should be added in liquid SiO2 composition is:
[0169]
[0170] —The volume of SiO2 in the liquid slag component that should be added at time t; —Density of liquid SiO2
[0171]
[0172] The working principle of this invention is:
[0173] Unlike the traditional method of adding pre-melted solid slag powder manually to the surface of the molten steel in the continuous casting process of iron and steel metallurgy, this method uses an external component melting system 8 to heat and melt the solid protective slag into groups separately to a liquid state, and then stores them in the corresponding liquid slag component storage system 10 for later use. Two component monitoring systems 21 are installed above the crystallizer 22 to monitor the changes in the composition of the liquid protective slag on the surface of the molten steel in the crystallizer 22 in real time. After summarizing the data from each composite system, the control system continuously calculates the composition of the liquid protective slag based on the principle of maintaining the constant proportion of each component before and after the reaction. Simultaneously, the control terminal controls the amount of specific components of the liquid slag to be replenished. The liquid slag storage system 10, in conjunction with the flow control system 11, first adds the component liquid slag to the mixing device 15 for thorough mixing via the liquid slag component conveying system 13. Then, through the mixing device outlet 17 and the liquid slag conveying system 18, the liquid slag is added in real time to the liquid slag layer on the surface of the molten steel in the crystallizer 22 via the liquid slag inlet 20. This maintains the "dynamic stability" of the protective slag components, thereby maintaining the stability of the protective slag viscosity, melting temperature, crystallization and heat transfer properties, ensuring the stable and smooth operation of the continuous casting process, and improving the quality of the cast billet.
[0174] It should be noted that, in this document, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, the phrase "comprising an element defined as..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.
[0175] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A method for dynamically controlling the composition of externally added liquid protective slag in continuous casting, comprising a device for dynamically controlling the composition of externally added liquid protective slag in continuous casting, the device including a control terminal (23), characterized in that, The control terminal (23) is equipped with a crystallizer (22), which is fitted with several component monitoring systems (21) and several liquid sludge inlet ports (20). The crystallizer (22) is fitted with an immersion port (19). The upper side of the crystallizer (22) is equipped with a composite system ⑤. The composite system ⑤ is connected to the liquid sludge inlet ports (20) through a liquid sludge conveying system (18). The upper side of the composite system ⑤ is equipped with several composite systems ①. The lower side of the composite system ① is equipped with composite systems ②, ③ and ④ in sequence. The composite system ⑤ is connected to the composite system ④. Includes the following steps: 1) The control terminal (23) will receive various types of information collected from composite system ①, composite system ②, composite system ③, composite system ④, and composite system ⑤ in real time; 2) The control terminal (23) will summarize the various information collected in real time by each composite system and calculate the amount of a certain component of the liquid slag to be added at that time. 3) The method for dynamic control of the composition of the external liquid protective slag in continuous casting obtains the amount of a certain liquid slag component to be added at different times by continuously calculating the changes in the content of each component of the protective slag at different times. The method for dynamically controlling the composition of external liquid protective slag in continuous casting, which replenishes the "consumed components" of the liquid slag, is based on the principle of maintaining the proportion of each component unchanged before and after the reaction of the liquid protective slag. 4) The control terminal (23) will transmit the calculation results to composite system ①, composite system ②, composite system ③, composite system ④, and composite system ⑤ in real time; 5) The composite systems ①, ②, ③, ④, and ⑤ will receive instructions and automatically control each system component to complete the specified operation; 6) The composite systems ①, ②, ③, ④ and ⑤ will feed back the instruction execution information to the control terminal in real time (23). 7) The composite system ①, composite system ②, composite system ③, composite system ④, and composite system ⑤ are closely coordinated with the control terminal (23) to replenish the required liquid slag components to the liquid slag layer on the steel surface of the crystallizer (22) in real time to maintain the "dynamic stability" of the protective slag components. 8) Maintain the stability of the viscosity, crystallization and heat transfer properties of the protective slag to ensure the stable and smooth operation of the continuous casting process; Step 3) includes the following steps: First, the analytical expression for the change of protective slag consumption over time in the continuous casting process is established as follows: ; In the formula: Q 渣 -Contains flux consumption, kg; a—Length of the upper section of the crystallizer, mm; b—Width of the upper section of the crystallizer, mm; ξ—Cross-sectional shape velocity coefficient, m·mm·min -1 ρ—density of liquid protective slag, g·cm³ -3 ;l max —Effective length of crystallizer, m; K 凝固 — Solidification coefficient of molten steel in the crystallizer, mm·min -0.5 f—crystallizer vibration frequency, min -1 η—viscosity of liquid protective slag, Pa·s; ν—pulling speed, m·min -1 c—length of the lower section of the crystallizer, mm; d—width of the lower section of the crystallizer, mm; δ—shell thickness of the billet when it exits the crystallizer, mm; L—casting length of the billet, m; t—continuous casting time, min; Then, the changes in the components in the liquid protective slag were determined; Finally, the calculation and analysis of the addition amount of each component of the liquid protective slag at different times were performed. Determining the changes in each component in the liquid protective slag in the above steps includes: Determination of CaO mass percentage content: ; In the formula: w(CaO) t % —CaO content in the liquid protective slag at time t; w(CaO) 0 % —Initial CaO content of the liquid protective slag; Q 渣 -Consumable amount of protective slag, kg; M 总 —Total mass of liquid protective slag added to the crystallizer at the initial moment, kg; t—Continuous casting time, min; Determination of SiO2 mass percentage content: ; In the formula: w(SiO2) t % —SiO2 content of the liquid protective slag at time t; w(SiO2) 0 % —Initial SiO2 content of liquid protective slag; β—Mass transfer coefficient, m·s; A—Phase interface area, m 2 ρ—density of liquid protective slag, g·cm³ -3 n—dimensionless coefficient, 33-35 for ordinary steel, 42-45 for high-quality steel; V—volume of the fluid, m³ 3 t—continuous casting time, in minutes; Determination of Al2O3 mass percentage content: ; In the formula: w (Al2O3) t % —Al2O3 content in the liquid protective slag at time t; w(Al2O3) 0 % —Al2O3 content at the initial moment of the liquid protective slag; w(SiO2) 0 % —Initial SiO2 content of liquid protective slag; β—Mass transfer coefficient, m·s; A—Phase interface area, m 2 ρ—density of liquid protective slag, g·cm³ -3 n—dimensionless coefficient, 33-35 for ordinary steel, 42-45 for high-quality steel; V—volume of the fluid, m³ 3 t—continuous casting time, min; Q 渣 -Consumable amount of protective slag, kg; M 总 —Total mass of liquid protective slag added to the crystallizer at the initial moment, kg; t—Continuous casting time, min; The calculation and analysis of the amount of each component added to the liquid protective slag at different times in the above steps includes: Record the composition w(CaO) in the initial protective slag. 0 % :w(SiO2) 0 % :w(Al2O3) 0 % =p:q:k, and after the reaction reaches time t, record the component w (CaO) in the protective slag. t % :w(SiO2) t % :w(Al2O3) t % =p t :q t :k t Based on the principle of maintaining the composition of the liquid protective slag unchanged, the following relationship exists in the reaction of the steel slag up to time t: p:q:k=(p t +x):(q t +y):k t =(pk t ):(qk t ):(kk t If w(CaO) is present in the protective slag at time t, then... % The amount added is x=pk t -p t ,Right now: ; In the formula: x - the amount of w (CaO) to be added to the protective slag from continuous casting to time t. % p - The simplest proportion of initial CaO in the three components CaO, SiO2, and Al2O3 in the protective slag; w(Al2O3) 0 % —Al2O3 content at the initial moment of the liquid protective slag; w(SiO2) 0 % —Initial SiO2 content of liquid protective slag; β—Mass transfer coefficient, m·s; A—Phase interface area, m 2 ρ—density of liquid protective slag, g·cm³ -3 n—dimensionless coefficient, 33-35 for ordinary steel, 42-45 for high-quality steel; V—volume of the fluid, m³ 3 t—continuous casting time, min; w (CaO) 0 % —Initial CaO content of the liquid protective slag; Q 渣 -Consumable amount of protective slag, kg; M 总 —Total mass of the liquid protective slag added to the crystallizer at the initial moment, kg; At time t, w(SiO2) in the protective slag % The amount added is y=qk t -q t ,Right now: ; In the formula: y - the amount of w (SiO2) to be added to the protective slag from continuous casting to time t. % ;q - the simplest proportion of initial SiO2 in the three components CaO, SiO2, and Al2O3 in the protective slag; w(Al2O3) 0 % —Al2O3 content at the initial moment of the liquid protective slag; w(SiO2) 0 % —Initial SiO2 content of liquid protective slag; Q 渣 -Consumable amount of protective slag, kg; M 总 —Total mass of liquid protective slag added to the crystallizer at the initial moment, kg; t—Continuous casting time, min; β—Mass transfer coefficient, m·s; A—Phase interface area, m² 2 ρ—density of liquid protective slag, g·cm³ -3 n—dimensionless coefficient, 33-35 for ordinary steel, 42-45 for high-quality steel; V—volume of the fluid, m³ 3 t—continuous casting time, min.
2. The method for dynamically controlling the composition of externally added liquid protective slag in continuous casting according to claim 1, characterized in that... The composite system ① includes a hopper (1), which is located above the composite system ⑤. An automatic feeding system (2) is installed at the bottom of the hopper, and an automatic weighing system (3) is installed on the lower side of the automatic feeding system (2). The automatic weighing system (3) transmits weighing data information to the control terminal (23).
3. The method for dynamically controlling the composition of externally added liquid protective slag in continuous casting according to claim 2, characterized in that... The composite system ② includes a component conveying device (4), which is located on the lower side of the automatic weighing system (3). A dust cover (6) is installed on the lower side of the component conveying device (4), and a component transport pipe (5) is installed between the dust cover (6) and the component conveying device (4).
4. The method for dynamic control of the composition of externally added liquid protective slag in continuous casting according to claim 3, characterized in that... The composite system ③ includes a component melting system (8), which is located on the lower side of the dust cover (6). The feed end of the component melting system (8) is connected to the dust cover (6). A support column (7) is installed outside the component melting system (8). A motor rotation system (9) is installed outside the component melting system (8). The motor rotation system (9) is connected to the support column (7).
5. The method for dynamic control of the composition of externally added liquid protective slag in continuous casting according to claim 4, characterized in that... The composite system ④ includes a liquid slag component storage system (10), which is located outside the component melting system (8). A flow control system (11) is installed on the liquid slag component storage system (10). The flow control system (11) is connected to the composite system ⑤ through the liquid slag component conveying system (13). A temperature control system (12) is installed inside the liquid slag component storage system (10).
6. The method for dynamic control of the composition of externally added liquid protective slag in continuous casting according to claim 5, characterized in that... The composite system ⑤ mixing device (15) is located on the lower side of the liquid slag component storage system (10). The mixing device (15) is provided with a mixing inlet (14), which is connected to the liquid slag component conveying system (13). The mixing device (15) is equipped with a mixing parameter setting terminal (16). The mixing device (15) is provided with a mixing outlet (17) on its lower side, which is connected to the liquid slag conveying system (18).
Citation Information
Patent Citations
Casting powder adding device for continuous casting crystallizer and operation method thereof
CN102642002B
Automatic feeding device for casting powder
CN218168651U
Method and device for improving surface quality of cast blank of continuous casting machine by adding covering slag
CN105750519A
Continuous casting powder repeated distributing and adding device
CN218361973U