A method for treating the surface of a ceramic membrane gasket
By restoring the surface condition of the ceramic film pad through heat treatment and polishing, the problem of the pad adhering to the support was solved, the pad could be reused, production costs were reduced, and the pass rate of the support was improved.
Patent Information
- Application Number
- CN202410497344.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-24
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-04-24
AI Technical Summary
After long-term use, ceramic film pads tend to adhere to the support blank, causing the support blank to tear or develop indentation defects, resulting in significant waste, failing to guarantee the pass rate of the support, and increasing production costs.
By heat-treating and polishing the ceramic film pad, its surface condition is restored, oil film and hard particles are removed, the porous structure is restored, the load-bearing requirements of the support blank are met, and qualified pads are screened for reuse by monitoring the diagonal deformation.
It effectively reduces pad waste, lowers production costs, improves the pass rate of the support, extends the service life of the pad, and meets the load-bearing requirements of the support.
Smart Images

Figure CN118386117B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of ceramic membrane production technology, and in particular to a method for surface treatment of ceramic membrane pads. Background Technology
[0002] Ceramic membranes have numerous advantages, including high separation efficiency, stable performance, good chemical stability, resistance to acids and alkalis, resistance to organic solvents, antibacterial properties, high temperature resistance, antifouling properties, high mechanical strength, good regeneration performance, simple separation process, low energy consumption, easy operation and maintenance, and long service life. They have been successfully applied in many fields such as food, beverage, plant (medicine) deep processing, biomedicine, fermentation, and fine chemicals.
[0003] Currently, the preparation process of ceramic membranes includes extrusion, spraying, and sintering. During the extrusion of the support preform, a sponge board (composed of a metal support frame and sponge pads, etc.) is required as a backing. However, the cutting effect is poor after continuous extrusion of the support preform on the sponge board, resulting in sponge board fragments remaining connected, and the yield rate of the ceramic membrane support is also low. Furthermore, the sponge board is prone to damage during long-term use, with a limited service life, requiring replacement every 2-3 months, directly contributing to the consistently high production cost of ceramic membranes. Therefore, the applicant has designed a method for preparing ceramic splicing plates using ceramic membrane waste as the main raw material (see "A Method for Preparing Ceramic Splicing Plates Using Ceramic Membrane Waste and the Ceramic Splicing Plate", Publication No.: CN116477923A, Publication Date: 2023-07-25), replacing the traditional sponge board as a backing with a ceramic splicing plate.
[0004] However, the aforementioned pads have revealed new problems after long-term use. For example, the pads tend to stick to the support blanks, causing them to tear when removed, or the support blanks develop obvious indentation defects after drying. Discarding these pads directly would be wasteful, incur transportation costs, and pollute the environment, contradicting the environmental protection goals of companies. Continuing to use them would compromise the pass rate of the supports. Summary of the Invention
[0005] This invention addresses the problems of waste and inability to guarantee the pass rate of existing support plates by providing a ceramic film plate surface treatment method. The method involves heat treatment and polishing the plate to restore its surface condition for reuse, thereby meeting the load-bearing requirements of the support blank. This method also reduces waste, lowers production costs, and helps ensure the pass rate of the support.
[0006] The technical solution adopted in this invention is: A method for surface treatment of a ceramic film pad includes the following steps: Step S1: Perform initial screening on the rectangular pads, retain the repairable pads, and measure the initial diagonal dimensions R1, R2, R3, and R4 of the four diagonals on both sides of the pads. Among them, the repairable pad must meet the requirement that the length and width of the area on the pad that effectively supports the support blank are greater than the length and width of the support blank, and the surface of the pad must be free of cracks, protrusions, depressions and holes that are visible to the naked eye. Step S2: Place the pad retained in step S1 into the kiln for heat treatment; Step S3: Polish the pad after heat treatment in step S2 and remove surface dust. Step S4: Measure the diagonal dimensions R1', R2', R3' and R4' of the four diagonals on both sides of the pad after polishing in step S3, and calculate the deformation amounts ΔL1, ΔL2, ΔL3 and ΔL4 of the corresponding four diagonals on both sides of the same pad after heat treatment and polishing. If any one of the deformation amounts ΔL1, ΔL2, ΔL3, and ΔL4 exceeds the threshold Q, then it is discarded; If the deformation amounts ΔL1, ΔL2, ΔL3, and ΔL4 are all ≤ the threshold Q, they are retained and reused for ceramic membrane production. in, ; ; ; .
[0007] Furthermore, in step S2, when the pad is placed in the kiln, it is placed on the silicon carbide kiln plate by laying a single piece flat or stacking multiple pieces in multiple rows.
[0008] Furthermore, in step S2, when the pads are placed on the silicon carbide kiln plate in a multi-layer, multi-column stacking manner, the maximum number of layers in a single column does not exceed 10.
[0009] Furthermore, in step S2, the heat treatment temperature is 650±20℃.
[0010] Furthermore, in step S2, the temperature is raised to 650±20℃ using a gradient heating method, held at that temperature, and then cooled down along with the furnace.
[0011] Furthermore, in step S2, during the gradient heating, the temperature is first increased to 150°C at a rate of 5~10°C / min, then increased to 450°C at a rate of 3~5°C / min, and finally increased to 650±20°C at a rate of 1~3°C / min.
[0012] Furthermore, in step S2, the heat preservation time is 80~120 minutes.
[0013] Furthermore, in step S4, the threshold Q = 1.5‰.
[0014] The beneficial effects of this invention are: This invention provides a method for surface treatment of ceramic film pads. By heat-treating and polishing the pads, the surface condition of the pads is restored, allowing them to be reused and meet the load-bearing requirements of the support blank. This method also reduces waste, lowers production costs, and helps ensure the pass rate of the support. Attached Figure Description
[0015] Figure 1 This is a schematic flowchart of the surface treatment method for the ceramic film pad in the embodiment.
[0016] Figure 2 Burning curve for removing oil film from the pad.
[0017] Figure 3 This is a SEM image of the surface of the pad before heat treatment, magnified at 1000x.
[0018] Figure 4 This is a SEM image of the surface of the pad before heat treatment, magnified at 2000x.
[0019] Figure 5 This is a SEM image of the surface of the pad before heat treatment, magnified at 5000x.
[0020] Figure 6 The image shows the surface of the pad before heat treatment at a magnification of 20,000.
[0021] Figure 7 This is a SEM image of the surface of the pad after heat treatment and polishing, magnified at 1000x.
[0022] Figure 8 This is a SEM image of the surface of the pad after heat treatment and polishing, magnified at 2000x.
[0023] Figure 9 This is a SEM image of the surface of the pad after heat treatment and polishing, magnified at 5000x.
[0024] Figure 10 This is a SEM image of the surface of the pad after heat treatment and polishing, magnified at 20,000x. Detailed Implementation
[0025] The specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings.
[0026] A method for surface treatment of ceramic film pads, the process of which is shown in the attached figure. Figure 1 As shown in the figure. The surface treatment method for the ceramic film pad includes the following steps: Step S1: Perform initial screening on the rectangular pads, retain the repairable pads, and measure the initial diagonal dimensions R1, R2, R3, and R4 of the four diagonals on both sides of the pads. Among them, the repairable pad must meet the requirement that the length and width of the area on the pad that effectively supports the blank of the support body are greater than the length and width of the blank of the support body, and the surface of the pad must be free of cracks, protrusions, depressions and holes that are visible to the naked eye.
[0027] Step S2: Place the pad retained in step S1 into the kiln for heat treatment.
[0028] The ceramic membrane support green body is mainly composed of alumina powder, pore-forming agent, binder, lubricant, dispersant, and water, which are extruded together. When the support green body is placed on the pad, trace amounts of water, pore-forming agent, binder, lubricant, and dispersant migrate into the porous structure of the pad. When the support green body and the pad are simultaneously dried in an environment of 85-95℃ for a long period, a sticky oil film forms on the surface of the pad. After the oil film forms, it blocks the porous structure of the pad surface, preventing further absorption of moisture. As a result, the support green body sticks to the pad during extrusion, leading to its scrapping. Furthermore, due to the influence of the production process and storage environment, hard particles (such as support fragments, hard ceramic powder, alumina powder, etc.) easily adhere to the surface of the pad, making wiping difficult and causing indentation defects in the support green body. At the same time, hard particles further exacerbate the blockage of the oil film on the pad surface. The sticky nature of the oil film means that conventional polishing methods are not effective in removing the oil film from the pad surface. Therefore, through extensive testing in this embodiment, it was found that the oil film can be destroyed by subjecting the gasket to high-temperature heat treatment, thereby restoring the porous structure of the gasket surface.
[0029] In this embodiment, the pads are placed on the silicon carbide kiln plate using either a single flat layer or multiple layers stacked in multiple rows. If multiple layers are used, the maximum number of layers per row does not exceed 10. When the maximum number of layers is 11 or more, the overall heat treatment time will be prolonged, and energy consumption will increase. Furthermore, because too many layers prevent heat from being transferred to the interior of the pads during heat treatment, it affects the degree of damage to the oil film structure and also hinders the evaporation of moisture adsorbed within the pads.
[0030] Meanwhile, through long-term testing, this embodiment demonstrates that setting the heat treatment temperature to 650±20℃ results in a superior overall treatment effect, duration, and energy consumption. Furthermore, to ensure the effectiveness of the heat treatment and facilitate oil film structure disruption and moisture evaporation, this embodiment employs a gradient heating method to raise the temperature to 650±20℃, hold it at that temperature for 80~120 minutes, and then cool it down with the furnace. Specifically, the gradient heating first raises the temperature to 150℃ at a rate of 5~10℃ / min, then to 450℃ at a rate of 3~5℃ / min, and finally to 650±20℃ at a rate of 1~3℃ / min.
[0031] Step S3: Polish the pad after heat treatment in step S2 and remove surface dust.
[0032] In this embodiment, after the pad has undergone heat treatment, the oil film structure is destroyed. Polishing and grinding at this point can completely remove the oil film from the pad's surface. After polishing and grinding, a high-pressure air gun is used to blow away surface dust and restore the porous structure of the pad's surface.
[0033] Step S4: Measure the diagonal dimensions R1', R2', R3' and R4' of the four diagonals on both sides of the pad after polishing in step S3, and calculate the deformation amounts ΔL1, ΔL2, ΔL3 and ΔL4 of the corresponding four diagonals on both sides of the same pad after heat treatment and polishing. If any one of the deformation amounts ΔL1, ΔL2, ΔL3, and ΔL4 exceeds the threshold Q (e.g., threshold Q = 1.5‰), then it is discarded. If the deformation amounts ΔL1, ΔL2, ΔL3, and ΔL4 are all ≤ the threshold Q, they are retained and reused for ceramic membrane production. in, ; ; ; .
[0034] After one or more repeated heat treatments, the pad itself will also undergo a certain degree of deformation. Therefore, in this embodiment, to prevent excessive deformation from affecting the pass rate of the support, the deformation of the diagonal dimension of the pad is monitored, and pads with deformation within the threshold Q are retained.
[0035] The ceramic film pad surface treatment method in this embodiment restores the surface condition of the pad by heat treatment and polishing, allowing it to be reused and meet the load-bearing requirements of the support blank. At the same time, it can reduce waste and reduce production costs, and help ensure the qualification rate of the support.
[0036] The following is a more specific example to illustrate this. Example
[0037] A method for surface treatment of a ceramic membrane pad, comprising the following steps: 1. Perform initial screening on rectangular pads. Unusable pads are selected separately. The remaining pads are measured along the four diagonals on both sides, stacked neatly on a special pallet, and labeled. 2. According to the kiln loading requirements, stack the pads in 4 layers neatly on the flat silicon carbide kiln plate. After inspection and approval, put them into the kiln and close the kiln door. 3. Follow the "Firing Curve for Removing Oil Film from the Pad" (as attached). Figure 2 As shown, the kiln curve needs to be entered, then the kiln is started and fired according to the curve. After the curve is fired, it is cooled to 100°C and removed from the kiln. During this process, the pads are fired in the kiln and kept at a constant temperature for a certain period of time, which removes the moisture absorbed by the pads and burns off the oil film on the pads. 4. After exiting the kiln, the pads are transported to a designated location and polished using a polishing machine equipped with polishing pads. High-pressure air guns are used to blow away hard particles from the surface. 5. Use a standard ruler to check the diagonal dimensions of the pad. If the diagonal deformation is no more than 1.5‰, it can be used in production; if it is greater than 1.5‰, it should be scrapped.
[0038] In this embodiment, the SEM results of the surface of the pad before heat treatment are shown in the attached figure. Figures 3-6 As shown in the attached figure. The SEM results of the surface of the pad after heat treatment and polishing are also shown. Figures 7-10 As shown in the figure, the porous structure of the pad is almost invisible on the surface before heat treatment, but it is restored after heat treatment and polishing. That is, by using the ceramic film pad surface treatment method in this embodiment, the pad can be restored to its initial state (a state without oil film adhesion) and can be reused.
[0039] The pads used for 7, 30, 60, and 90 days without treatment, as well as the pads treated with the method described in this embodiment after 90 days of continuous use, were used in the production process of ceramic membrane supports. The number and defect rate of defective products with surface cracks, warping, holes, breakage, bulging, etc., when producing 1000 supports (with the same composition and sintering process) were statistically analyzed. The statistical results are shown in Table 1 below.
[0040] Table 1 Statistical Results
[0041] Based on the above statistical results, the ceramic film pad surface treatment method in Example 1 can effectively remove the oil film adhering to the surface of the continuously used pad, allowing it to return to its initial state, which helps to reduce the defect rate during the production of the support.
Claims
1. A method for surface treatment of a ceramic film pad, characterized in that, Includes the following steps: Step S1: Perform initial screening on the rectangular pads, retain the repairable pads, and measure the initial diagonal dimensions R1, R2, R3, and R4 of the four diagonals on both sides of the pads. Among them, the repairable pad must meet the requirement that the length and width of the area on the pad that effectively supports the support blank are greater than the length and width of the support blank, and the surface of the pad must be free of cracks, protrusions, depressions and holes that are visible to the naked eye. Step S2: Place the pad retained in step S1 in the kiln for heat treatment at a temperature of 650±20℃. Specifically, the temperature is raised to 650±20℃ using a gradient heating method, held at that temperature, and then cooled down with the furnace. After heat treatment, the oil film that migrated to the pad during the drying process of the ceramic film support green body is destroyed, restoring the porous structure of the pad surface. Step S3: Polish the pad after heat treatment in step S2 and remove surface dust. Step S4: Measure the diagonal dimensions R1', R2', R3' and R4' of the four diagonals on both sides of the pad after polishing in step S3, and calculate the deformation amounts ΔL1, ΔL2, ΔL3 and ΔL4 of the corresponding four diagonals on both sides of the same pad after heat treatment and polishing. If any one of the deformation amounts ΔL1, ΔL2, ΔL3, and ΔL4 exceeds the threshold Q, then it is discarded; If the deformation amounts ΔL1, ΔL2, ΔL3, and ΔL4 are all ≤ the threshold Q, they are retained and reused in the production of ceramic membranes. in, ; ; ; 。 2. The surface treatment method for ceramic film pads according to claim 1, characterized in that, In step S2, when the pad is placed in the kiln, it is placed on the silicon carbide kiln plate by laying a single piece flat or stacking multiple pieces in multiple rows.
3. The surface treatment method for ceramic film pads according to claim 2, characterized in that, In step S2, when the pads are placed on the silicon carbide kiln plate in a multi-layer, multi-column stacking manner, the maximum number of layers in a single column does not exceed 10.
4. The surface treatment method for ceramic film pads according to claim 2, characterized in that, In step S2, the temperature is first increased to 150°C at a rate of 5-10°C / min, then increased to 450°C at a rate of 3-5°C / min, and finally increased to 650±20°C at a rate of 1-3°C / min.
5. The surface treatment method for ceramic film pads according to claim 1, characterized in that, In step S2, the heat preservation time is 80~120 minutes.
6. The method for surface treatment of ceramic film pads according to any one of claims 1 to 5, characterized in that, In step S4, the threshold Q = 1.5‰.
Citation Information
Patent Citations
Regeneration method of ceramic annular parts for semiconductor 8-inch wafer manufacturing thin film manufacturing procedure WxZ process
CN108816870A
Method for preparing ceramic connecting plate by utilizing ceramic membrane waste and ceramic connecting plate