Method for manufacturing porous ceramic and porous ceramic, atomizing core, electronic cigarette and medical device

By using carbon fiber and SiC ceramic deposition technology in the preparation process of porous ceramics, the problems of controllability and uniformity of pore structure of porous ceramic atomizing cores are solved, thereby improving atomization consistency and safety.

CN118388241BActive Publication Date: 2026-11-24品度生物科技(深圳)有限公司
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410557826.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-30
Publication Date
2026-11-24
Estimated Expiration
2044-04-30

AI Technical Summary

Technical Problem

The existing porous ceramic atomizing cores have poor controllability and uniformity of internal pore structure, resulting in poor atomization consistency and a risk of oil leakage or core clogging.

Method used

Using carbon fiber as a preform, a precursor and hydrogen are introduced into a chemical vapor infiltration furnace to carry out a deposition reaction. After depositing SiC ceramics, they are sintered to prepare porous ceramics, and the formation and distribution of pore structure are controlled.

Benefits of technology

The directional preparation of porous ceramic pore structures has been achieved, with good pore size and distribution uniformity, which improves atomization consistency, reduces the risk of oil leakage or core clogging, and enhances safety and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This application provides a method for preparing porous ceramics, as well as porous ceramics, atomizing cores, electronic cigarettes, and medical devices. The method for preparing porous ceramics includes: placing a preform with a grid structure in a chemical vapor infiltration furnace, introducing a precursor and hydrogen gas to carry out a deposition reaction, thereby depositing SiC ceramics on the surface of the preform and in the grid; after the deposition reaction, subjecting the preform with deposited SiC ceramics to a sintering reaction to remove the preform and prepare porous ceramics; wherein the deposition reaction temperature is 900℃-1050℃, and the time is 20h-40h; the preform includes carbon fibers; the precursor includes one or more of alkylsilanes and alkylchlorosilanes. This method can achieve the directional preparation of porous ceramic pore structures, and the pore size and distribution uniformity of the formed pore structure can be adjusted according to the preform. Simultaneously, the formed porous ceramics have strong mechanical properties, resulting in good atomization consistency when used as an atomizing core, reducing the risk of leakage or core clogging, and effectively improving safety and reliability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of ceramic preparation technology, and in particular to a method for preparing porous ceramics, as well as porous ceramics, atomizing cores, electronic cigarettes, and medical devices. Background Technology

[0002] An atomizer is a device that converts e-liquid into an aerosol, and it is widely used in medical devices and e-cigarettes. With the development of the e-cigarette industry, atomization technology and related materials are constantly being updated and iterated. Currently, the main atomization materials for e-cigarettes are cotton wicks and ceramic wicks. Cotton wicks are limited in application due to their poor oil retention, inconsistent quality, and tendency to spit out oil. To achieve stable and smooth flavor, porous ceramic atomizing wicks are often used to atomize e-liquid.

[0003] Currently, porous ceramic atomizing cores are mainly prepared by adding pore-forming agents to ceramic raw materials and then removing the pore-forming agents through sintering to form a porous structure. However, the controllability and uniformity of the internal pore structure of the ceramic atomizing core prepared by this method are poor, thus affecting the atomization consistency of the ceramic core. Summary of the Invention

[0004] Based on this, this application provides a method for preparing porous ceramics with better controllability of internal pore structure and uniformity of pore size distribution, as well as porous ceramics, atomizing cores, electronic cigarettes, and medical devices.

[0005] The first aspect of this application provides a method for preparing porous ceramics, comprising the following steps:

[0006] A preform with a grid structure is placed in a chemical vapor infiltration furnace, and a precursor and hydrogen are introduced to carry out a deposition reaction to deposit SiC ceramics on the surface of the preform and in the grid.

[0007] After the deposition reaction is completed, the preform after SiC ceramic deposition is subjected to a sintering reaction to remove the preform and prepare the porous ceramic.

[0008] The deposition reaction is carried out at a temperature of 900℃-1050℃ for 20h-40h; the preform includes carbon fiber; and the precursor includes one or more of alkylsilane and alkylchlorosilane.

[0009] In some embodiments, the precursor includes one or more of methyltrichlorosilane, dimethyldichlorosilane, isopropylsilane, and n-butylsilane.

[0010] In some embodiments, the volumetric flow rate ratio of the hydrogen to the precursor is (8-12):1.

[0011] In some embodiments, the deposition pressure is 3 kPa-8 kPa.

[0012] In some embodiments, the sintering reaction is carried out at a temperature of 650°C-750°C for a duration of 15-25 hours.

[0013] The second aspect of this application provides a porous ceramic, which is prepared using the preparation method of the first aspect of this application.

[0014] In some embodiments, the porosity of the porous ceramic is 50%-67%, and the maximum destructive force of the porous ceramic is ≥60N.

[0015] A third aspect of this application provides an atomizing core comprising a porous ceramic prepared by the preparation method of the first aspect of this application or a porous ceramic prepared by the second aspect of this application.

[0016] The fourth aspect of this application provides an electronic cigarette that includes the atomizing core of the third aspect of this application.

[0017] The fifth aspect of this application provides a medical device that includes the atomizing core of the third aspect of this application.

[0018] The above-mentioned method for preparing porous ceramics uses carbon fiber as a preform, then deposits SiC ceramics on the surface and in the mesh of the preform, and finally removes the preform by high-temperature oxidation to obtain porous ceramics. This method can achieve the directional preparation of porous ceramic pore structures. The pore size and distribution uniformity of the formed pore structure can be adjusted according to the preform. At the same time, the formed porous ceramics have strong mechanical properties, which makes them good atomization consistency when used as ceramic atomizing cores, reducing the risk of oil leakage or core clogging, and effectively improving safety and reliability. Detailed Implementation

[0019] To facilitate understanding of this application, a more complete description of the application will be provided below with reference to relevant embodiments. Preferred embodiments of the application are given below. However, the application can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a thorough and complete understanding of the disclosure of this application.

[0020] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application belongs. The terminology used herein is for the purpose of describing particular embodiments only and is not intended to be limiting of the application.

[0021] As used herein, the terms "and / or," "or / and," and "and / or" encompass any one of two or more of the related listed items, as well as any and all combinations of the related listed items. These arbitrary and all combinations include any two related listed items, any more related listed items, or a combination of all related listed items. It should be noted that when at least three items are connected using at least two conjunctions selected from "and / or," "or / and," and "and / or," it should be understood that, in this application, the technical solution undoubtedly includes solutions connected by "logical AND," and also undoubtedly includes solutions connected by "logical OR."

[0022] In this application, the technical features described in an open-ended manner include both closed technical solutions consisting of the listed features and open technical solutions that include the listed features.

[0023] In this application, numerical ranges are referred to as continuous unless otherwise specified, and include the minimum and maximum values ​​of the range, as well as every value between the minimum and maximum values. Furthermore, when the range refers to integers, it includes every integer between the minimum and maximum values ​​of the range. Additionally, when multiple ranges are provided to describe a feature or characteristic, the ranges may be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges to which they are incorporated.

[0024] This document only specifically discloses some numerical ranges. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, just as any upper limit can be combined with any other upper limit to form an unspecified range. Furthermore, each individually disclosed point or single value can itself serve as a lower or upper limit and be combined with any other point or single value or with other lower or upper limits to form an unspecified range.

[0025] Unless otherwise specified, the temperature parameters in this application may be either constant temperature processing or processing within a certain temperature range. The constant temperature processing allows temperature fluctuations within the precision range controlled by the instrument, such as ±5°C, ±4°C, ±3°C, ±2°C, or ±1°C.

[0026] In this document, the term "suitable" as used in phrases such as "suitable combination," "suitable method," and "any suitable method" refers to the ability to implement the technical solution of this application, solve the technical problem of this application, and achieve the expected technical effect of this application.

[0027] In this application, terms such as "further," "even more," and "particularly" are used for descriptive purposes and to indicate differences in content, but should not be construed as limiting the scope of protection of this application.

[0028] In this application, "optionally," "optionally," and "optional" mean that something is optional, that is, it means that it is selected from either "with" or "without." If there are multiple "optional" entries in a technical solution, unless otherwise specified, and there are no contradictions or mutual constraints, each "optional" entry shall be independent.

[0029] In the description of the application, "multiple" means at least two, such as two, three, etc., unless otherwise explicitly specified.

[0030] Unless otherwise specified, all embodiments and optional embodiments of this application can be combined to form new technical solutions. Unless otherwise specified, all technical features and optional technical features of this application can be combined to form new technical solutions.

[0031] Unless otherwise specified, all steps in this application may be performed sequentially or randomly, but sequentially is preferred.

[0032] Currently, the controllability and uniformity of the internal pore structure of the porous ceramic atomizing core used in e-cigarettes are poor, resulting in uneven oil conduction rate and poor atomization consistency, which may lead to oil leakage or burnt core.

[0033] The embodiments of this application provide a method for preparing porous ceramics, comprising the following steps:

[0034] A preform with a grid structure is placed in a chemical vapor infiltration furnace, and a precursor and hydrogen are introduced to carry out a deposition reaction to deposit SiC ceramics on the surface of the preform and in the grid. After the deposition reaction is completed, the preform after SiC ceramic deposition is subjected to a sintering reaction to remove the preform and prepare porous ceramics. The deposition reaction temperature is 900℃-1050℃ and the time is 20h-40h. The preform includes carbon fibers. The precursor includes one or more of alkylsilanes and alkylchlorosilanes.

[0035] Understandably, the above-mentioned method for preparing porous ceramics uses carbon fiber as a preform, then deposits SiC ceramics on the surface and in the mesh of the preform, and finally removes the preform by high-temperature oxidation to obtain porous ceramics. This method enables the directional preparation of porous ceramic pore structures, and the pore size and uniformity of the resulting pore structure can be adjusted according to the preform. Simultaneously, the resulting porous ceramics exhibit strong mechanical properties, resulting in good atomization consistency when used as an atomizing core, reducing the risk of oil leakage or core clogging, and effectively improving safety and reliability. Furthermore, compared to traditional irregular pore structures, the porous ceramics prepared using this method have the largest proportion of fibrous pores, making stress concentration less likely. The SiC framework and fibrous pores possess superior resistance to external stress damage, thereby improving the safety and reliability of the porous ceramics.

[0036] As an example, the deposition reaction temperature is 900℃-1050℃; for example, it can be, but is not limited to, 900℃, 910℃, 920℃, 930℃, 940℃, 950℃, 960℃, 970℃, 980℃, 990℃, 1000℃, 1010℃, 1020℃, 1030℃, 1040℃, 1050℃, or any range between two of the above temperatures. When the deposition reaction temperature is below the above range, the reaction rate is slow, and the obtained SiC grains are not fully fused and agglomerated to form continuous SiC, resulting in low ceramic strength; when the deposition reaction temperature is above the above range, the activation energy of surface diffusion is very high, and it is difficult for the SiC grains in the deposition process to fuse together, resulting in loose aggregates and low strength in the prepared porous ceramics.

[0037] As an example, the deposition reaction time is 20-40 hours; for example, it can be, but is not limited to, 20 hours, 22 hours, 24 hours, 26 hours, 28 hours, 30 hours, 32 hours, 34 hours, 36 hours, 38 hours, 40 hours, or any two of the above time ranges. When the deposition reaction time is shorter than the above range, the deposited SiC framework is incomplete, and the prepared porous ceramic has low strength; when the deposition reaction time is longer than the above range, the deposited SiC framework is thicker and more complete, and the framework strength is better; however, if the deposition time is too long, the porosity of the obtained porous ceramic will be too low, and if it is used to prepare ceramic atomizing core products, problems such as core clogging and poor oil circulation are likely to occur.

[0038] It should be noted that the temperature and time of the deposition reaction can be combined in any suitable way, and both can be selected from any deposition reaction temperature and time described in this article.

[0039] In some exemplary embodiments, the precursor includes one or more of methyltrichlorosilane, dimethyldichlorosilane, isopropylsilane, and n-butylsilane.

[0040] In some embodiments, the volumetric flow rate ratio of hydrogen to precursor is (8-12):1; for example, it can be, but is not limited to, 8:1, 8.5:1, 9:1, 9.5:1, 10:1, 10.5:1, 11:1, 11.5:1, 12:1, or any range between two of the above ratios. When the volumetric flow rate ratio of hydrogen to precursor is within the above range, it helps to completely decompose the precursor, resulting in SiC with high purity and good structural integrity and uniformity.

[0041] As one possible implementation, the deposition pressure is 3KPa-8KPa; for example, it can be, but is not limited to, 3KPa, 4KPa, 5KPa, 6KPa, 7KPa, 8KPa or any range between the two aforementioned deposition pressures.

[0042] In some embodiments, the sintering reaction temperature is 650℃-750℃; for example, it can be, but is not limited to, 650℃, 660℃, 670℃, 680℃, 690℃, 700℃, 710℃, 720℃, 730℃, 740℃, 750℃, or any range between two of the above temperatures.

[0043] In some embodiments, the sintering reaction time is 15h-25h; for example, it can be, but is not limited to, 15h, 16h, 17h, 18h, 19h, 20h, 21h, 22h, 23h, 24h, 25h or any range between two of the above times.

[0044] It should be noted that the temperature and time of the sintering reaction can be combined in any suitable way, and both can be selected from any sintering reaction temperature and time described in this article.

[0045] An embodiment of this application provides a porous ceramic, which is prepared using the aforementioned method for preparing porous ceramics.

[0046] In some embodiments, the porosity of the porous ceramic is 50%-67%; for example, it can be, but is not limited to, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, or any two of the above values. When the porosity of the porous ceramic is controlled within this range, the e-liquid conduction rate is sufficient, balancing the e-liquid atomization rate with the e-liquid conduction rate, resulting in the best flavor experience, while also preventing the atomizer coil from burning.

[0047] In some implementations, the maximum destructive force of the porous ceramic is ≥60N.

[0048] An embodiment of this application provides an atomizing core, the material of which includes porous ceramic prepared by the aforementioned porous ceramic preparation method or the aforementioned porous ceramic. The atomizing core, made of the aforementioned porous ceramic material, exhibits good atomization consistency, reduces the risk of oil leakage or core clogging, and offers high safety and reliability.

[0049] Embodiments of this application also provide an electronic cigarette that includes the aforementioned atomizing core.

[0050] Embodiments of this application also provide a medical device comprising the aforementioned atomizing core.

[0051] The technical solutions of this application will be described in detail below with reference to specific embodiments. It should be understood that these embodiments are only for illustrating this application and are not intended to limit the scope of this application. For experimental methods in the following embodiments where specific conditions are not specified, please refer to the guidelines given in this application first, or follow experimental manuals or conventional conditions in the field, or follow the conditions recommended by the manufacturer, or refer to experimental methods known in the field.

[0052] In the specific embodiments described below, the measurement parameters involving raw material components may have slight deviations within the weighing accuracy range unless otherwise specified. Temperature and time parameters are subject to acceptable deviations due to instrument testing accuracy or operational precision.

[0053] Example 1

[0054] Step S1: Select woven and uniformly sized carbon fibers as preforms and place the preforms in a chemical vapor infiltration furnace.

[0055] Step S2: Select methyltrichlorosilane (CH3SiCl3, MTS) as the precursor, pass flowing hydrogen gas, deposit SiC ceramic at a deposition pressure of 5 kPa and a temperature of 900 °C; wherein the volume flow ratio of hydrogen to methyltrichlorosilane is 10:1 and the deposition time is 20 h.

[0056] Step S3: After deposition, the preform with deposited SiC ceramic is placed in a box sintering furnace and held at 700°C in air for 20 hours to remove the preform and prepare the pore structure, thereby obtaining a porous ceramic with oriented fiber pore structure.

[0057] Example 2

[0058] Step S1: Select woven and uniformly sized carbon fibers as preforms and place the preforms in a chemical vapor infiltration furnace.

[0059] Step S2: Select methyltrichlorosilane (CH3SiCl3, MTS) as the precursor, pass flowing hydrogen gas, deposit SiC ceramic at a deposition pressure of 5 kPa and a temperature of 1000 °C; wherein the volume flow ratio of hydrogen to methyltrichlorosilane is 10:1, and the deposition time is 30 h.

[0060] Step S3: After deposition, the preform with deposited SiC ceramic is placed in a box sintering furnace and held at 700°C in air for 20 hours to remove the preform and prepare the pore structure, thereby obtaining a porous ceramic with oriented fiber pore structure.

[0061] Example 3

[0062] Step S1: Select woven and uniformly sized carbon fibers as preforms and place the preforms in a chemical vapor infiltration furnace.

[0063] Step S2: Select methyltrichlorosilane (CH3SiCl3, MTS) as the precursor, pass flowing hydrogen gas, deposit SiC ceramic at a deposition pressure of 5 kPa and a temperature of 1050 °C; wherein the volume flow ratio of hydrogen to methyltrichlorosilane is 10:1, and the deposition time is 20 h.

[0064] Step S3: After deposition, the preform with deposited SiC ceramic is placed in a box sintering furnace and held at 700°C in air for 20 hours to remove the preform and prepare the pore structure, thereby obtaining a porous ceramic with oriented fiber pore structure.

[0065] Example 4

[0066] Step S1: Select woven and uniformly sized carbon fibers as preforms and place the preforms in a chemical vapor infiltration furnace.

[0067] Step S2: Select methyltrichlorosilane (CH3SiCl3, MTS) as the precursor, pass flowing hydrogen gas, deposit SiC ceramic at a deposition pressure of 3 kPa and a temperature of 1000 °C; wherein the volume flow ratio of hydrogen to methyltrichlorosilane is 8:1, and the deposition time is 30 h.

[0068] Step S3: After deposition, the preform with deposited SiC ceramic is placed in a box sintering furnace and held at 650°C in air for 25 hours to remove the preform and prepare the pore structure, thereby obtaining a porous ceramic with an oriented fiber pore structure.

[0069] Example 5

[0070] Step S1: Select woven and uniformly sized carbon fibers as preforms and place the preforms in a chemical vapor infiltration furnace.

[0071] Step S2: Select methyltrichlorosilane (CH3SiCl3, MTS) as the precursor, pass flowing hydrogen gas, deposit SiC ceramic at a deposition pressure of 8 kPa and a temperature of 1050 °C; wherein the volume flow ratio of hydrogen to methyltrichlorosilane is 12:1, and the deposition time is 30 h.

[0072] Step S3: After deposition, the preform with deposited SiC ceramic is placed in a box sintering furnace and held at 750°C in air for 15 hours to remove the preform and prepare the pore structure, thereby obtaining a porous ceramic with an oriented fiber pore structure.

[0073] Example 6

[0074] Step S1: Select woven and uniformly sized carbon fibers as preforms and place the preforms in a chemical vapor infiltration furnace.

[0075] Step S2: Select dimethyldichlorosilane ((CH3)2SiCl2) as the precursor, pass flowing hydrogen gas, deposit SiC ceramic at a deposition pressure of 5 kPa and a temperature of 1000 °C; wherein the volume flow ratio of hydrogen to methyltrichlorosilane is 10:1, and the deposition time is 30 h.

[0076] Step S3: After deposition, the preform with deposited SiC ceramic is placed in a box sintering furnace and held at 700°C in air for 20 hours to remove the preform and prepare the pore structure, thereby obtaining a porous ceramic with oriented fiber pore structure.

[0077] Comparative Example 1

[0078] Step S1: Select 75 parts of SiC powder, 10 parts of glass powder, and 15 parts of PS microspheres, put them into a three-dimensional mixer and mix for 2 hours, and dry at 120℃ for 2 hours to obtain solid powder.

[0079] Step S2: Place 15 parts paraffin wax, 3 parts stearic acid and 7 parts beeswax in a wax machine at 100°C and heat to melt. Then add solid powder and stir to obtain wax slurry.

[0080] Step S3: Place the wax slurry in the molding equipment, place the pre-made heating component in the mold, and then die-cast to obtain the product wax blank;

[0081] Step S4: Place the wax blank with powder in an air furnace to remove wax at a temperature of 700℃ for 2 hours.

[0082] Step S5: Remove the powder from the porous ceramic semi-finished product after wax removal, wash it with ultrasonic water for 20 minutes, and then dry it in an oven at 120℃ for 2 hours.

[0083] Step S6: The dried porous ceramic semi-finished product is sintered at high temperature to obtain the porous ceramic finished product. The sintering temperature is 900℃ and the holding time is 3h.

[0084] Comparative Example 2

[0085] Step S1: Dry the above raw materials, select 80 parts of SiC powder, 10 parts of glass powder, and 10 parts of PS microspheres, put them into a three-dimensional mixer and mix for 2 hours, and dry at 120°C for 2 hours to obtain solid powder.

[0086] Step S2: Place 30 parts paraffin wax, 3 parts stearic acid and 5 parts beeswax in a wax machine at 100°C and heat to melt. Then add the solid powder and stir to obtain a wax slurry.

[0087] Step S3: Place the wax slurry in the molding equipment, place the pre-made heating component in the mold, and then die-cast to obtain the product wax blank;

[0088] Step S4: Place the wax blank with powder in an air furnace to remove wax at a temperature of 700℃ for 2 hours.

[0089] Step S5: Remove the powder from the porous ceramic semi-finished product after wax removal, wash it with ultrasonic water for 20 minutes, and then dry it in an oven at 120℃ for 2 hours.

[0090] Step S6: The dried porous ceramic semi-finished product is sintered at high temperature to obtain the porous ceramic finished product. The sintering temperature is 1000℃ and the holding time is 2h.

[0091] Comparative Example 3

[0092] The difference between Comparative Example 3 and Example 2 is that the deposition reaction temperature in step S2 of Comparative Example 3 is 1100°C, while all other conditions are the same. Step S2 is as follows:

[0093] Step S2: Select methyltrichlorosilane (CH3SiCl3, MTS) as the precursor, pass flowing hydrogen gas, deposit SiC ceramic at a deposition pressure of 5 kPa and a temperature of 1100 °C; wherein the volume flow ratio of hydrogen to methyltrichlorosilane is 10:1, and the deposition time is 30 h.

[0094] Comparative Example 4

[0095] The difference between Comparative Example 4 and Example 2 is that the deposition reaction temperature in step S2 of Comparative Example 4 is 850°C, while all other conditions are the same. Step S2 is as follows:

[0096] Step S2: Select methyltrichlorosilane (CH3SiCl3, MTS) as the precursor, pass flowing hydrogen gas, deposit SiC ceramic at a deposition pressure of 5 kPa and a temperature of 850 °C; wherein the volume flow ratio of hydrogen to methyltrichlorosilane is 10:1 and the deposition time is 30 h.

[0097] Comparative Example 5

[0098] The difference between Comparative Example 5 and Example 2 is that the deposition reaction time in step S2 of Comparative Example 5 is 45 hours, while all other steps are the same. Step S2 is as follows:

[0099] Step S2: Select methyltrichlorosilane (CH3SiCl3, MTS) as the precursor, pass flowing hydrogen gas, deposit SiC ceramic at a deposition pressure of 5 kPa and a temperature of 1000 °C; wherein the volume flow ratio of hydrogen to methyltrichlorosilane is 10:1 and the deposition time is 45 h.

[0100] Comparative Example 6

[0101] The difference between Comparative Example 6 and Example 2 is that the deposition reaction time in step S2 of Comparative Example 6 is 15 hours, while all other steps are the same. Step S2 is as follows:

[0102] Step S2: Select methyltrichlorosilane (CH3SiCl3, MTS) as the precursor, pass flowing hydrogen gas, deposit SiC ceramic at a deposition pressure of 5 kPa and a temperature of 1000 °C; wherein the volume flow ratio of hydrogen to methyltrichlorosilane is 10:1, and the deposition time is 15 h.

[0103] The porous ceramics prepared in the above embodiments and comparative examples were subjected to porosity tests and maximum destructive force tests, and the test methods are as follows:

[0104] 1. Porosity testing method: The porosity is determined by the Archimedes method. The initial dry mass, saturated water weight, and saturated air weight of the sample are measured by a porosity analyzer. The porosity can be calculated from these data.

[0105] 2. Maximum destructive force test method: The test is conducted using an electronic universal testing machine. A 50mm diameter disc is selected, and the ceramic sample is placed horizontally on the disc. Pressure is applied from the start until the product is destroyed. The test speed is 50mm / min, and the pressure value that can be withstood is recorded.

[0106] The porosity and strength test results of the porous ceramics in the above embodiments and comparative examples are shown in Table 1.

[0107] Table 1

[0108]

[0109] As can be seen from the results of Examples 1-6 and Comparative Examples 1-6 in Table 1, the porous ceramics prepared by the preparation method of this application have suitable porosity and high mechanical strength.

[0110] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0111] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this patent application should be determined by the appended claims.

Claims

1. A method for producing a porous ceramic, characterized by, Includes the following steps: A preform with a grid structure is placed in a chemical vapor infiltration furnace, and a precursor and hydrogen are introduced to carry out a deposition reaction to deposit SiC ceramics on the surface of the preform and in the grid. After the deposition reaction is completed, the preform after SiC ceramic deposition is subjected to high temperature treatment to remove the preform and prepare the porous ceramic. The deposition reaction is carried out at a temperature of 900℃-1050℃ for 20h-40h and at a deposition pressure of 3KPa-8KPa. The preform includes carbon fiber. The precursor includes one or more of alkylsilane and alkylchlorosilane. The volume flow rate ratio of hydrogen to the precursor is (8-12):

1. The high-temperature treatment is carried out at a temperature of 650℃-750℃ for 15h-25h.

2. The production method according to claim 1, wherein The precursor includes one or more of methyltrichlorosilane, dimethyldichlorosilane, isopropylsilane, and n-butylsilane.

3. A porous ceramic, characterized by, It is prepared by the preparation method described in any one of claims 1 to 2.

4. The porous ceramic of claim 3, wherein, The porosity of the porous ceramic is 50%-67%, and the maximum destructive force of the porous ceramic is ≥60N.

5. An atomizing core characterized by, The atomizing core is made of porous ceramic as described in claim 3 or 4.

6. An electronic cigarette, characterized by Includes the atomizing core as described in claim 5.

7. A medical device, characterized by Includes the atomizing core as described in claim 5.

Citation Information

Patent Citations

  • Method for preparing highly-oriented perforated porous SiC ceramic material

    CN102173853A

  • Method for preparing porous silicon carbide ceramic based on template

    CN105237034A

  • Preparation method of silicon carbide porous ceramic atomizing core

    CN117209284A