A method for preparing high-strength tin-based babbitt alloy laser cladding layer with hot substrate
By using laser cladding technology and hot substrates in an inert gas atmosphere to prepare high-strength tin-based Babbitt alloy coatings, the problems of low thickness, complex processes, and low interfacial bonding strength in existing Babbitt alloy coating processing have been solved. This has enabled the preparation of efficient, multi-layer, high-strength Babbitt alloy coatings, improving interfacial bonding strength and wear resistance.
Patent Information
- Application Number
- CN202410498996.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-24
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-04-24
AI Technical Summary
Existing Babbitt alloy coating processes suffer from problems such as low single-layer forming thickness, complex procedures, low processing efficiency, low interfacial bonding strength, and high cost. In particular, traditional casting methods are prone to defects, while spraying and powder feeding additive manufacturing processes are complex and costly. Wire feeding laser cladding requires tin plating of the substrate, and single-layer cladding layers have weak subsequent machining capabilities.
A method for preparing a high-strength tin-based Babbitt alloy laser cladding layer using a hot substrate is proposed. By using laser cladding technology in an inert gas atmosphere, combined with preheating of the substrate material and multi-layer cladding, the tin-coating process is eliminated, forming a metallurgical bond to enhance the interface strength, thereby achieving a high-thickness and high-strength Babbitt alloy cladding layer.
It significantly improves the interfacial shear strength of the Babbitt alloy cladding layer, refines the grains, reduces processing steps, improves production efficiency, enhances the wear resistance and durability of the cladding layer, and achieves an interfacial bonding strength three times that of traditional methods, supporting the preparation of multi-layer high-thickness coatings.
Smart Images

Figure HDA0004808098700000011 
Figure HDA0004808098700000012 
Figure HDA0004808098700000021
Abstract
Description
Technical Field
[0001] This application belongs to the field of laser cladding processing, and specifically relates to a method for preparing a high-strength tin-based Babbitt alloy laser cladding layer using a hot substrate. Background Technology
[0002] Laser cladding is a process that involves adding external materials to a substrate after laser irradiation, either simultaneously or pre-placed, to form a molten pool, which then rapidly solidifies to create a coating layer. Its key features include low dilution but strong adhesion, exhibiting a metallurgical bond with the substrate. This significantly improves the wear resistance, corrosion resistance, heat resistance, oxidation resistance, and electrical properties of the substrate material, achieving surface modification and meeting specific performance requirements while saving substantial material costs. Compared to welding, spraying, electroplating, and vapor deposition, laser cladding offers advantages such as low dilution, dense structure, excellent coating-substrate adhesion, suitability for a wide range of cladding materials, and versatility in particle size and content.
[0003] Babbitt alloy, invented by the American Babbitt, is also known as white alloy. Its main components are tin, antimony, and copper. It is a low-melting-point bearing alloy with hard particle phases distributed in a soft matrix. Due to the good plasticity and low hardness of the soft matrix, it possesses excellent embedding, conformability, and anti-galling properties. During friction, the soft matrix wears down, while the hard particles remain to provide support, creating tiny gaps between the sliding surfaces. These gaps act as oil reservoirs and lubricating channels, resulting in excellent oil-jetting performance. Babbitt alloy, with its anti-friction properties, is the only material suitable for rotation relative to low-hardness shafts. Compared to other bearing materials, it has better adaptability and press-fit properties. Due to its low coefficient of thermal expansion, good thermal conductivity, corrosion resistance, and excellent anti-friction performance, it is widely used in large marine diesel engines, turbines, alternators, as well as other mining machinery and large rotating machinery.
[0004] Traditional Babbitt alloy coatings are mostly produced using a casting process, employing static casting to cover the surface of the substrate material. The traditional static casting method mainly involves steps such as cleaning and tinning the substrate, melting the alloy, casting, and cooling. This process is complex, and the Babbitt alloy layer is prone to defects such as coarse grains, compositional segregation, cracks, shrinkage cavities, slag pits, and peeling, severely affecting the performance of the Babbitt alloy. Furthermore, the casting process involves significant heat input, leading to noticeable thermal deformation of the workpiece during machining. Besides traditional casting, there are also spraying, coating, and welding methods, but these processes do not significantly improve the wear resistance, hardness, and bonding strength of Babbitt alloy to the substrate. Recently, laser cladding technology has emerged for manufacturing Babbitt alloy coatings; however, existing powder-feeding additive manufacturing processes are complex, requiring multiple forming processes for low single-layer thicknesses, and existing wire-feeding processes have low strength and lack processes for preparing multi-layer, high-thickness coatings.
[0005] A laser additive manufacturing method for tin-based Babbitt alloy is disclosed in invention patent publication number CN107803501A. This method achieves the preparation of a cladding material layer on the surface of Babbitt alloy by combining low laser power, small layer thickness, and substrate preheating. However, in order to achieve the preparation of a high-thickness coating, this process adopts a small-layer, multi-layer stacked cladding technique, which increases the preparation steps of the cladding layer, increases the complexity of the process, and increases the process cost.
[0006] A method for laser cladding of Babbitt alloy is disclosed in the invention patent with publication number CN114875402A. However, in order to ensure the interface bonding strength, the substrate material still needs to be tinned. In addition, it is only a single-layer cladding process, and the resulting Babbitt alloy cladding layer is low, resulting in weak subsequent machining capability.
[0007] In summary, existing powder-fed laser cladding technology for Babbitt alloy surfaces suffers from drawbacks such as low single-layer thickness, complex processes, and low processing efficiency. Furthermore, the use of powder materials leads to harsh working conditions and high costs. Existing wire-fed laser cladding technology still requires tin plating of the substrate material, making the process complex and limiting its ability to form a single-layer laser cladding layer, resulting in weak subsequent machining capabilities. Moreover, among all processing methods, the highest interfacial shear strength of the formed Babbitt alloy layer is only about 140 MPa, severely impacting the service life of the Babbitt alloy coating. Summary of the Invention
[0008] The purpose of this invention is to propose a method for preparing a high-strength tin-based Babbitt alloy laser cladding layer using a hot substrate. This method overcomes the shortcomings of existing technologies and solves problems such as low interfacial bonding strength, complex processes, low production efficiency, and harsh working conditions for workers in traditional casting, spraying, arc welding, and powder feeding additive manufacturing processes. By keeping the substrate hot before cladding, the surface tinning process is eliminated, and the interfacial bonding strength is enhanced through metallurgical bonding, thus achieving the preparation of a thick, high-strength Babbitt alloy cladding layer. This results in the efficient preparation of a high-wear-resistant and high-durability Babbitt alloy cladding layer.
[0009] To achieve the above technical objectives, the present invention is implemented through the following technical solution:
[0010] A method for preparing a high-strength tin-based Babbitt alloy laser cladding layer using a hot substrate includes the following steps: Step 1: Surface treatment of the substrate material processing surface and the Babbitt alloy wire; Step 2: Heating the substrate to 40-70℃; Step 3: Irradiating the Babbitt alloy wire with a laser irradiation device under an inert gas atmosphere, causing the Babbitt alloy wire to melt part of the substrate material, forming a mixed molten pool, where the Fe portion of the substrate material melts into the Babbitt alloy and solidifies together to form a Babbitt alloy cladding layer, controlling the movement trajectory of the laser irradiation device relative to the substrate material so that the overlap rate between the Babbitt alloy cladding layers formed on adjacent movement trajectories is 20%-40%; Step 4: After cooling the workpiece with the surface clad in Babbitt alloy to room temperature, restarting the laser irradiation device, irradiating the Babbitt alloy wire under an inert gas atmosphere, simultaneously melting part of the surface Babbitt alloy cladding layer to form a mixed molten pool, and forming a multi-layer Babbitt alloy cladding layer after the molten pool solidifies.
[0011] The base material is any one of plain carbon steel plate Q235, Q245 or Q345, and the Babbitt alloy wire is composed of antimony 3% to 15%, copper 2% to 6%, cadmium <1%, with the balance being tin and unavoidable impurities.
[0012] The surface treatment method in step one is as follows: the oxide layer on the surface of the substrate material to be processed is removed by grinding, and the surface of the Babbitt wire and the substrate material to be processed is cleaned with acetone or ethanol.
[0013] In step two, the heating method for the hot substrate is any one or a combination of two or more of the following: heating platform, hot air blowing, and baking lamp irradiation.
[0014] In step three, the laser irradiation device moves at a speed of 5-20 mm / s relative to the substrate material, the laser power used is 1200-4000W, the diameter of the Babbitt alloy wire is 1-3 mm, and the wire feeding speed of the Babbitt alloy wire is 1-5 m / min.
[0015] In step three, the laser irradiation device moves at a speed of 10-40 mm / s relative to the substrate material, the laser power used is 1000-3000 W, the diameter of the Babbitt alloy wire is 1-3 mm, and the wire feeding speed of the Babbitt alloy wire is 1-5 m / min.
[0016] The inert gas is argon or nitrogen, and the concentration of the inert gas in the laser cladding part is not less than 95%.
[0017] Partial melting refers to melting thickness not exceeding 1 / 2 of the original cladding layer thickness.
[0018] The laser irradiation device includes a laser emitting head and a wire feeding mechanism. The laser emitting head is vertically arranged and connected to the laser via an optical fiber. The wire feeding mechanism is connected to one side of the laser emitting head via a fixing frame. The direction of the molten wire of the wire feeding mechanism forms an angle of 30-60° with the direction of laser emission. The intersection of the molten wire and the laser is located 1-5mm above the intersection of the laser and the substrate.
[0019] An inert gas tube is connected to the other side of the laser emitter. One end of the inert gas tube exits above the cladding zone, and the other end of the inert gas tube is connected to a gas cylinder.
[0020] Compared with the prior art, the beneficial effects achieved by the present invention are as follows:
[0021] 1) Laser cladding produces a uniform distribution of white blocky, triangular or polygonal tin-antimony compounds and white blocky, needle-like or dot-like copper-tin compounds in the metallographic structure of tin-based Babbitt alloy. The maximum diameter of the reinforcing phase does not exceed 15 μm. The grains and reinforcing phases of the Babbitt alloy cladding layer are significantly refined, and the hardness and wear resistance are significantly improved.
[0022] 2) By heating the substrate, the laser-clad tin-based Babbitt alloy coating exhibits a clear metallurgical bond at the interface with the substrate, free from defects such as pores and cracks. Simultaneously, due to the addition of a heated substrate, Fe from the substrate diffuses into the tin-based Babbitt alloy coating, forming intermetallic compounds, effectively enhancing the interfacial strength of the Babbitt alloy coating. Compared to existing laser cladding technologies, its interfacial shear strength is increased by approximately 20 MPa. The Babbitt alloy layer and the workpiece substrate form a dense metallurgical bond, with a bonding strength approximately three times that of traditional statically cast Babbitt alloy layers.
[0023] 3) The laser cladding technology used in this application has a large single-layer forming thickness, which reduces the processing steps and has high production efficiency. In addition, compared with the existing research on wire feeding additive manufacturing technology, it can prepare multi-layer cladding layers with a maximum thickness of over 20mm, which improves the subsequent machining capability while ensuring the interface bonding strength. Attached Figure Description
[0024] Figure 1 This is a schematic diagram of the working state of the laser irradiation device according to an embodiment of the present invention;
[0025] Figure 2 This is a comparison diagram of the average size of the laser cladding layer and the cast Babbitt alloy reinforced phase in Embodiment 1 of the present invention;
[0026] Figure 3 This is a comparison diagram of the microhardness of the laser cladding layer and the cast Babbitt alloy in Embodiment 1 of the present invention;
[0027] Figure 4 This is a scanning electron microscope image of the Babbitt alloy cladding layer in Embodiment 1 of the present invention;
[0028] Figure 5 This is a surface scan of the Fe element in the Babbitt alloy cladding layer in Embodiment 1 of the present invention;
[0029] Figure 6 This is a surface scan of the Sn element in the Babbitt alloy cladding layer in Embodiment 1 of the present invention;
[0030] Figure 7 This is the interfacial shear curve of the Babbitt alloy cladding layer in Embodiment 1 of the present invention;
[0031] Figure 8 This is a scanning electron microscope image of the Babbitt alloy cladding layer in Embodiment 2 of the present invention;
[0032] Figure 9 This is the interfacial shear curve of the Babbitt alloy cladding layer in Embodiment 2 of the present invention;
[0033] Figure 10 This is a scanning electron microscope image of the Babbitt alloy cladding layer in Embodiment 3 of the present invention;
[0034] Figure 11 This is the interfacial shear curve of the Babbitt alloy cladding layer in Embodiment 3 of the present invention;
[0035] Figure 12 This is a scanning electron microscope image of the Babbitt alloy cladding layer in the comparative example;
[0036] Figure 13 The interface shear curves of the Babbitt alloy cladding layer in the comparative example are shown.
[0037] Figure 14 These are comparison diagrams showing the interfacial bonding strength of Babbitt alloy cladding layers prepared by Examples 1-3 of the present invention, the comparative examples, and different preparation methods. Detailed Implementation
[0038] The technical solution of the present invention will be clearly and completely described below with reference to specific embodiments. Obviously, the described embodiments are some embodiments of the present invention, but not all embodiments.
[0039] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the specific embodiments used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the specific embodiments described below are some embodiments of the present invention. For those skilled in the art, other specific embodiments can be obtained based on these specific embodiments without creative effort.
[0040] The components of the embodiments of the invention described and shown in the specific embodiments herein can be arranged and designed in countless different configurations. Therefore, the following detailed description of the embodiments of the invention provided in the specific embodiments is not intended to limit the scope of the claimed invention, but merely to illustrate selected embodiments of the invention.
[0041] See Figure 1 The laser irradiation device includes a laser emitting head and a wire feeding mechanism. The laser emitting head is vertically positioned and connected to the laser via an optical fiber. The wire feeding mechanism is connected to one side of the laser emitting head via a mounting bracket. The direction of the molten wire in the wire feeding mechanism forms a 45° angle with the laser emission direction, and the intersection of the molten wire and the laser is located 1-5 mm above the intersection of the laser and the substrate. An inert gas tube is connected to the other side of the laser emitting head. One end of the inert gas tube exits above the cladding zone, and the other end is connected to a gas cylinder.
[0042] Example 1
[0043] In Example 1, the specific composition of the Babbitt alloy wire used is: Sb: 11.29wt%, Cu: 6.03wt%, Fe: 0.029wt%, As: 0.002wt%, balance Sn, and the matrix material is Q235.
[0044] A method for preparing a high-strength tin-based Babbitt alloy laser cladding layer using a hot substrate includes the following steps:
[0045] Step 1: Perform surface treatment on both the substrate material's machined surface and the Babbitt wire. First, grind the substrate material to remove the surface adsorption and oxide layers. Then, clean the machined surface and the Babbitt wire with ethanol or acetone to remove surface oil and contaminants. This step increases the adhesion between the cladding material and the substrate material, preventing defects such as interface inclusions, porosity, coating dilution, and peeling.
[0046] Step 2: Heat the substrate to 50°C;
[0047] Step 3: Under an inert gas atmosphere, irradiate the Babbitt alloy wire with a laser irradiation device. This melts part of the base material, forming a mixed molten pool. The Fe portion of the base material melts into the Babbitt alloy, and both solidify together to form a Babbitt alloy cladding layer. Control the movement trajectory of the laser irradiation device relative to the base material, ensuring an overlap rate of 20%-40% between adjacent Babbitt alloy cladding layers formed on their respective trajectories. The laser irradiation device moves relative to the base material along a set trajectory. This movement can be formed by the movement of the laser irradiation device itself, the movement of the base material, or the simultaneous and superimposed movement of both the base material and the laser irradiation device.
[0048] The process parameters for the first layer of Babbitt alloy cladding are as follows: laser power: 2000W, scanning speed: 0.5m / min, wire feed speed: 2m / min, the distance between the shielding gas outlet and the laser spot is approximately 15mm, the laser spot diameter is 2mm, the Babbitt alloy wire diameter is 1.6mm, the overlap rate between two adjacent laser weld beads is 30%, and the angle between the wire feed direction and the laser irradiation direction is 30-60°; the single layer thickness is approximately 3mm.
[0049] Step 4: After cooling the workpiece with the Babbitt alloy cladding layer to room temperature, restart the laser irradiation device. In an inert gas atmosphere, the laser irradiation device irradiates the Babbitt alloy wire, simultaneously melting part of the surface Babbitt alloy cladding layer to form a mixed molten pool. After the molten pool solidifies, a multi-layer Babbitt alloy cladding layer is formed. The process parameters for processing the second and subsequent Babbitt alloy cladding layers are as follows: laser power: 1600W, scanning speed: 1m / min, wire feed speed: 2m / min, distance between the shielding gas outlet and the laser spot approximately 15mm, laser spot diameter 2mm, Babbitt alloy wire diameter 1.6mm, overlap rate between adjacent laser weld beads 40%, and angle between the wire feed direction and the laser irradiation direction 30-60°.
[0050] A comparison of the average size and microhardness of laser-clad Babbitt alloy and cast Babbitt alloy reinforced phases is shown in the figure below. Figure 2 , Figure 3 As shown. The microstructure of the obtained Babbitt alloy cladding layer is as follows. Figure 4 As shown in the figure, there are obvious metallurgical bonding traces at the interface, and significant intermetallic compounds diffused into the Babbitt alloy cladding layer. Compositional analysis reveals that the intermetallic compounds are composed of Sn and Fe. The presence of these dispersed hard intermetallic compounds at the interface leads to an increase in interface strength, approximately 20 MPa higher than that of existing Babbitt alloy powder feeding additive manufacturing methods. The interface shear curve is shown below. Figure 7 As shown.
[0051] Example 2
[0052] In Example 2, the specific composition of the Babbitt alloy wire used is: Sb: 11.29wt%, Cu: 6.03wt%, Fe: 0.029wt%, As: 0.002wt%, balance Sn, and the matrix material is Q245.
[0053] The surface treatment of the substrate material and Babbitt wire involves first grinding the substrate material to remove the surface adsorption and oxide layers, and then cleaning the surface to be processed and the Babbitt wire with ethanol or acetone to remove surface oil and adhering substances. This step can increase the adhesion between the cladding material and the substrate material and avoid defects such as interface inclusions, porosity, coating dilution, and peeling.
[0054] The laser irradiation device moves relative to the substrate material along a predetermined trajectory. This movement can be caused by the movement of the laser irradiation device itself, the movement of the substrate material, or the combined movement of both the substrate material and the laser irradiation device.
[0055] The substrate preheating temperature is 40℃; the process parameters for the first Babbitt alloy cladding layer are as follows: laser power: 2100W, scanning speed: 0.5m / min, wire feed speed: 2m / min, the distance between the protective gas outlet and the laser spot is approximately 15mm, the laser spot diameter is 2mm, the Babbitt alloy wire diameter is 1.6mm, the overlap rate between two adjacent laser weld beads is 30%, and the angle between the wire feed direction and the laser irradiation direction is 30-60°; in this example, the single-layer processing thickness is approximately 3mm.
[0056] The process parameters for the second and subsequent Babbitt alloy cladding layers are as follows: laser power: 1600W, scanning speed: 1m / min, wire feed speed: 2m / min, distance between the shielding gas outlet and the laser spot: approximately 15mm, laser spot diameter: 2mm, Babbitt alloy wire diameter: 1.6mm, overlap rate between adjacent laser weld beads: 40%, and angle between the wire feed direction and the laser irradiation direction: 30-60°. The thickness of each Babbitt alloy cladding layer after the second layer is approximately 2mm. This example can manufacture laser cladding layers with a total thickness exceeding 20mm.
[0057] The microstructure of the obtained Babbitt alloy cladding layer is as follows Figure 8 As shown in the figure, there are obvious metallurgical bonding traces at the interface, and significant intermetallic compounds diffused into the Babbitt alloy cladding layer. The presence of the interface strengthening phase results in a higher interface strength than the comparative example without a hot substrate. Its interface shear curve is shown in the figure. Figure 9 As shown.
[0058] Example 3
[0059] In Example 3, the specific composition of the Babbitt alloy wire used is: Sb: 11.29wt%, Cu: 6.03wt%, Fe: 0.029wt%, As: 0.002wt%, balance Sn, and the matrix material is Q245.
[0060] The surface treatment of the substrate material and Babbitt wire involves first grinding the substrate material to remove the surface adsorption and oxide layers, and then cleaning the surface to be processed and the Babbitt wire with ethanol or acetone to remove surface oil and adhering substances. This step can increase the adhesion between the cladding material and the substrate material and avoid defects such as interface inclusions, porosity, coating dilution, and peeling.
[0061] The laser irradiation device moves relative to the substrate material along a predetermined trajectory. This movement can be caused by the movement of the laser irradiation device itself, the movement of the substrate material, or the combined movement of both the substrate material and the laser irradiation device.
[0062] The substrate preheating temperature is 60℃. The process parameters for the first Babbitt alloy cladding layer are: laser power: 1900W, scanning speed: 0.5m / min, wire feed speed: 2m / min, distance between the shielding gas outlet and the laser spot approximately 15mm, laser spot diameter 2mm, Babbitt alloy wire diameter 1.6mm, overlap rate between adjacent laser weld beads 30%, and angle between the wire feed direction and the laser irradiation direction 30-60°. The process parameters for the second and subsequent Babbitt alloy cladding layers are: laser power: 1600W, scanning speed: 1m / min, wire feed speed: 2m / min, distance between the shielding gas outlet and the laser spot approximately 15mm, laser spot diameter 2mm, Babbitt alloy wire diameter 1.6mm, overlap rate between adjacent laser weld beads 40%, and angle between the wire feed direction and the laser irradiation direction 30-60°. In this example, the thickness of a single layer is approximately 3mm.
[0063] The microstructure of the obtained Babbitt alloy cladding layer is as follows Figure 10 As shown in the figure, there are obvious metallurgical bonding traces at the interface, and significant intermetallic compounds diffused into the Babbitt alloy cladding layer. Compared with the comparative example, coarse metallic compounds are clearly visible. Since Fe and Sn intermetallic compounds are brittle materials, excessive Fe and Sn compounds are more likely to cause crack propagation and fracture. However, the positive effects of these intermetallic compounds outweigh the negative effects of brittle phase aggregation, and the interface strength is still higher than that of the comparative example without a hot substrate. The interface shear curve is shown in the figure. Figure 11 As shown.
[0064] Comparative Example
[0065] The specific composition of the Babbitt alloy wire in this comparative example is: Sb: 11.29wt%, Cu: 6.03wt%, Fe: 0.029wt%, As: 0.002wt%, balance Sn, and the matrix material is Q235.
[0066] The substrate temperature is ambient temperature; no heating is applied. Other conditions are the same as in the previous embodiment.
[0067] Comparative microstructure of Babbitt alloy cladding layer interface such as Figure 12 As shown in the figure. Due to the low substrate temperature, Fe diffusion was minimal during the cladding layer preparation process, and no intermetallic compounds were formed at the interface that penetrated deep into the molten pool. Therefore, the interface strength was significantly affected, as shown in the interface shear strength curve. Figure 13 As shown.
[0068] Comparison of interfacial bonding strength of Babbitt alloy cladding layers prepared by different known methods is shown in the figure below. Figure 14 As shown, the interfacial shear strength of the Babbitt alloy cladding layer in Examples 1-3 is relatively high.
[0069] It should be noted that the above implementation methods are only used to illustrate the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the embodiments, those skilled in the art should understand that various combinations, modifications, or equivalent substitutions of the technical solutions of the present invention do not depart from the spirit and scope of the technical solutions of the present invention and should be covered within the scope of the claims of the present invention.
Claims
1. A method for preparing a high-strength tin-based Babbitt alloy laser cladding layer using a hot substrate, characterized in that: Includes the following steps: Step 1: Perform surface treatment on the machined surface of the base material and the Babbitt alloy wire respectively; the base material is any one of plain carbon steel plate Q235, Q245 or Q345, and the composition of the Babbitt alloy wire is antimony 3%~15%, copper 2%~6%, cadmium <1%, and the balance is tin and unavoidable impurities; Step 2: Heat the substrate to 40-70℃; Step 3: Under an inert gas atmosphere, irradiate the Babbitt alloy wire with a laser irradiation device to melt part of the base material, forming a mixed molten pool. The Fe portion of the base material melts into the Babbitt alloy and solidifies together to form a Babbitt alloy cladding layer. Control the movement trajectory of the laser irradiation device relative to the base material so that the overlap rate between the Babbitt alloy cladding layers formed on adjacent movement trajectories is 20%-40%. The movement speed of the laser irradiation device relative to the base material is 5-20 mm / s, the laser power used is 1200-4000 W, the diameter of the Babbitt alloy wire is 1-3 mm, and the wire feeding speed of the Babbitt alloy wire is 1-5 m / min. Step 4: After cooling the workpiece with the surface clad with Babbitt alloy to room temperature, restart the laser irradiation device. In an inert gas atmosphere, the laser irradiation device irradiates the Babbitt alloy wire, causing partial melting of the surface Babbitt alloy cladding layer to form a mixed molten pool. After the molten pool solidifies, a multi-layer Babbitt alloy cladding layer is formed. The partial melting refers to a melting thickness that is no more than 1 / 2 of the thickness of the surface Babbitt alloy cladding layer. The laser irradiation device includes a laser emitting head and a wire feeding mechanism. The laser emitting head is vertically arranged and connected to the laser via an optical fiber. The wire feeding mechanism is connected to one side of the laser emitting head via a fixing frame. The direction of the molten wire of the wire feeding mechanism forms an angle of 30-60° with the direction of laser emission. The intersection of the molten wire and the laser is located 1-5mm above the intersection of the laser and the substrate.
2. The method for preparing a high-strength tin-based Babbitt alloy laser cladding layer using a hot substrate according to claim 1, characterized in that, The surface treatment method in step one is as follows: the oxide layer on the surface of the substrate material to be processed is removed by grinding, and then the Babbitt wire and the surface of the substrate material to be processed are cleaned with acetone or ethanol.
3. The method for preparing a high-strength tin-based Babbitt alloy laser cladding layer using a hot substrate according to claim 1, characterized in that, In step two, the heating method for the hot substrate is any one or a combination of two or more of the following: heating platform, hot air blowing, and baking lamp irradiation.
4. The method for preparing a high-strength tin-based Babbitt alloy laser cladding layer using a hot substrate according to claim 1, characterized in that, The inert gas is argon or nitrogen, and the concentration of the inert gas in the laser cladding part is not less than 95%.
5. The method for preparing a high-strength tin-based Babbitt alloy laser cladding layer using a hot substrate according to claim 1, characterized in that, An inert gas tube is connected to the other side of the laser emitter. One end of the inert gas tube exits above the cladding zone, and the other end of the inert gas tube is connected to a gas cylinder.
Citation Information
Patent Citations
Laser additive manufacturing method for stannum-based babbitt alloy component
CN107803501A
Babbitt metal laser cladding processing method and laser cladding piece
CN114875402A