V-shaped bidirectional promoting highly ordered mesoporous WO3 / CeO2 catalyst, its preparation method and application
By adjusting the ratio of Ce and W, a V-driven bidirectional highly ordered mesoporous WO₃/CeO₂ catalyst was prepared, which solved the problems of low-temperature activity and biotoxicity of existing NH₃-SCR catalysts and achieved the ability of efficient low-temperature denitrification and resistance to complex working conditions.
Patent Information
- Application Number
- CN202410368540.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-28
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-03-28
AI Technical Summary
Existing NH₃-SCR catalysts have shortcomings in terms of low-temperature activity and biotoxicity, making it difficult to maximize adsorption and reaction performance simultaneously.
By adjusting the ratio of Ce and W, VO-Ce and VOW sites are formed, and a V bidirectional promoting highly ordered mesoporous WO₃/CeO₂ catalyst is prepared, which enhances its surface acidity and redox performance.
It significantly improves the low-temperature denitrification performance and water and sulfur resistance, making it suitable for low-temperature flue gas purification and providing a novel and efficient thermal catalyst application solution.
Smart Images

Figure CN118403627B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical fields of air pollution control technology and environmental functional materials, specifically relating to a V-bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst, its preparation method, and its application. Background Technology
[0002] Nitrogen oxides (NO) x NOx is considered one of the most dangerous air pollutants, causing serious air pollution problems such as photochemical smog, haze, and acid rain. Driven by tightening policies and increased environmental awareness, efforts are underway to achieve NOx targets. x To achieve efficient elimination of NO, various technologies have been developed, such as selective non-catalytic reduction of NO. x (SNCR), selective catalytic reduction of NO by urea or ammonia x (Urea-SCR or NH3-SCR), etc. Among them, NO x The NH3-SCR process achieves the highest efficiency, and a highly efficient catalyst is the core of NH3-SCR technology. To date, the most popular commercial NH3-SCR catalyst is V2O5-WO3(MoO3) / TiO2, which exhibits excellent denitrification efficiency and satisfactory resistance to SO2 poisoning at 300-400℃. However, the relatively poor low-temperature activity and biotoxicity of vanadium-based catalysts have prompted researchers to seek an NH3-SCR catalyst with excellent low-temperature activity and high vanadium utilization.
[0003] Researchers generally agree that effective adsorption and rapid surface reaction are important requirements for effective active sites in catalysts. However, maximizing both functions simultaneously remains a challenge. Summary of the Invention
[0004] To address the shortcomings of existing technologies, the present invention aims to provide a method for preparing a V-promoted highly ordered mesoporous WO3 / CeO2 catalyst. This method involves adjusting the ratio of Ce to W to form VO-Ce and VOW sites and enhancing the surface acidity and redox properties of the V-promoted highly ordered mesoporous WO3 / CeO2 catalyst, thereby significantly improving its adsorption and reaction performance.
[0005] Another object of the present invention is to provide a V-bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst obtained by the above preparation method, wherein the V-bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst is a low-V-loaded, V-bidirectionally promoted, highly ordered mesoporous thermal catalyst.
[0006] Another objective of this invention is to provide the application of the above-mentioned V-bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst in the removal of nitrogen oxides. The V-bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst has highly efficient and selective catalytic reduction removal of NO in flue gas, is suitable for low-temperature removal of nitrogen oxides, and can be applied in actual industrial flue gas purification treatment.
[0007] The objective of this invention is achieved through the following technical solution.
[0008] A method for preparing a V-type bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst includes the following steps:
[0009] Step 1: Mix cerium salt and water until homogeneous to obtain solution A. Mix solution A with KIT-6 template agent and stir until the solution evaporates to dryness to obtain a first solid. Grind the first solid into powder, calcine at 400-500℃ for 4-6 hours, cool to room temperature, wash, and dry to obtain mesoporous CeO2. The ratio of cerium salt to KIT-6 template agent by mass is (3-4.5):1.5.
[0010] In step 1, stirring until the solution evaporates includes: first stirring at 20-30°C at 500-700 rpm for 18-30 hours, and then stirring at 60-80°C at 500-700 rpm until the solution evaporates.
[0011] In step 1, the ratio of the mass fraction of the KIT-6 template agent to the volume fraction of water is 1.5:(30-50), where the mass fraction is in g and the volume fraction is in mL.
[0012] In step 1, the washing process involves first washing with an aqueous sodium hydroxide (NaOH) solution to remove the KIT-6 template agent, followed by washing with water until neutral. The concentration of sodium hydroxide in the aqueous sodium hydroxide (NaOH) solution is 1.8–3 mol / L.
[0013] In step 1, the drying temperature is 80-100℃ and the drying time is 20-24 hours.
[0014] Step 2: Mix the mesoporous CeO2 and solution B, stir until the solution evaporates to dryness to obtain a second solid, grind the second solid into powder, dry it, calcine it at 400-500℃ for 4-6 hours, and cool it to room temperature to obtain a highly ordered mesoporous WCe catalyst, wherein solution B is ammonium metatungstate hydrate ((NH4)2). 10 W 12 O 41 A mixture of xH2O), oxalic acid, and water, in which, by molar amount, Ce and ammonium metatungstate hydrate ((NH4)) are present in the mesoporous CeO2.10 W 12 O 41 The tungsten content in the metatungstate hydrate ((NH4)) is (0.8–0.95):(0.05–0.2) by molar fraction. 10 W 12 O 41 The ratio of xH2O to oxalic acid is 1:(1~3);
[0015] In step 2, the method for obtaining solution B is as follows: ammonium metatungstate hydrate ((NH4)2) 10 W 12 O 41 Mix xH2O and oxalic acid aqueous solution, and stir for 30-60 minutes until homogeneous to obtain solution B. The stirring speed is 500-700 rpm.
[0016] In step 2, the drying temperature is 80-100℃, and the drying time is 20-24 hours.
[0017] In step 2, stirring until the solution evaporates includes: first stirring at 20-30°C at 500-700 rpm for 6-24 hours, and then stirring at 60-80°C at 500-700 rpm until the solution evaporates.
[0018] Step 3: Mix the WCe highly ordered mesoporous catalyst with water, sonicate to obtain a WCe suspension, add an aqueous solution of ammonium metavanadate (NH4VO3) dropwise to the WCe suspension, sonicate, stir until the solution evaporates to dryness to obtain a third solid, grind the third solid into powder, dry it, calcine it at 400-500℃ for 4-6 hours, and cool it to room temperature to obtain a V bidirectional promoting highly ordered mesoporous WO3 / CeO2 catalyst, wherein, by mass parts, the ratio of ammonium metavanadate to the WCe highly ordered mesoporous catalyst in the aqueous solution of ammonium metavanadate (NH4VO3) is 1:100.
[0019] In step 3, the ultrasound duration is 30–60 min and the ultrasound frequency is 30–50 kHz.
[0020] In step 3, the drying temperature is 80-100℃ and the drying time is 20-24h.
[0021] In step 3, the ratio of the mass fraction of the WCe highly ordered mesoporous catalyst to the volume fraction of water in step 3 is 0.3:(30-50), where the mass fraction is in g and the volume fraction is in mL.
[0022] In step 3, the concentration of ammonium metavanadate in the aqueous solution of ammonium metavanadate (NH4VO3) is 1-3 mg / mL.
[0023] In steps 1 to 3, the heating rate to 400 to 500°C is 0.5 to 1°C / min.
[0024] In step 3, stirring until the solution evaporates includes: first stirring at 20-30°C at a speed of 500-700 rpm for 6-24 hours, and then stirring at 60-80°C at a speed of 500-700 rpm until the solution evaporates.
[0025] The method for preparing the KIT-6 template agent in the above technical solution includes the following steps:
[0026] S1, water, hydrochloric acid, and polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer (P123) are mixed and stirred until homogeneous to obtain a first mixture. The first mixture is then mixed with sodium dodecyl sulfate (SDS) until homogeneous to obtain a second mixture. Under stirring conditions, tetraethyl orthosilicate (TEOS) is added dropwise to the second mixture, and the mixture is stirred and reacted for at least 24 hours to obtain a third mixture. The ratio of polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer (P123), sodium dodecyl sulfate (SDS), and tetraethyl orthosilicate (TEOS) by mass is 12:1.38:25.8.
[0027] In S1, water, hydrochloric acid, and polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer (P123) are mixed and stirred at a speed of 300-400 rpm until homogeneous to obtain a first mixture.
[0028] In S1, the first mixture and sodium dodecyl sulfate (SDS) are stirred at 30°C for at least 6 hours to achieve homogeneity, thereby obtaining the second mixture.
[0029] In S1, under stirring conditions of 700-800 rpm, tetraethyl orthosilicate (TEOS) is added dropwise to the second mixture, and the mixture is stirred at 400-500 rpm for at least 24 hours to obtain the third mixture.
[0030] In S1, the ratio of water, hydrochloric acid and polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer (P123) by mass parts is 312:144:12.
[0031] In S1, the concentration of HCl in the hydrochloric acid is 2 mol / L.
[0032] S2, the third mixture is hydrothermally heated at 100°C for 22-26 hours, cooled to room temperature to obtain a first precipitate, the first precipitate is washed, dried, ground, and calcined at 550°C for 5-6 hours to obtain KIT-6 template agent.
[0033] In S2, the heating rate to 550°C is 1°C / min.
[0034] In S2, water is used for washing.
[0035] The V-promoted highly ordered mesoporous WO3 / CeO2 catalyst obtained by the above preparation method.
[0036] The above-mentioned V-bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst is used for the removal of nitrogen oxides.
[0037] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0038] 1. This invention leverages the highly ordered pore structure and large specific surface area of KIT-6 template agent (KIT-6 mesoporous material), which are suitable for the dispersion of active sites. Mesoporous CeO2 is prepared via a reverse template method, followed by the preparation of a highly ordered mesoporous WCe catalyst via an impregnation method. Finally, a V-bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst is synthesized via ammonium metavanadate impregnation and calcination. Compared with common VW / TiO2 and WCe catalysts, the V-bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst significantly enhances low-temperature denitrification performance (at GHSV = 120,000 h⁻¹). -1 Under high gas velocity ratios, it maintains a denitrification conversion rate of over 95% within a temperature range of 225-400℃, and exhibits excellent water and sulfur resistance (at a low temperature of 200℃ and GHSV = 120,000 h). -1 At high gas velocity ratios, the V-driven highly ordered mesoporous WO3 / CeO2 catalyst exhibits significantly better resistance to water and sulfur, and is more capable of withstanding complex operating conditions. The V-driven highly ordered mesoporous WO3 / CeO2 catalyst of this invention, after the introduction of trace amounts of V, shows greatly enhanced surface acidity and redox properties, thus exhibiting excellent catalytic activity. This invention proposes the advantages of V-driven bidirectional promotion and regulation of the V coordination environment in practical applications, providing a new approach for the development of novel high-efficiency thermocatalysts.
[0039] 2. This invention addresses the problem of NO in low-temperature flue gas from glass factories, cement plants, and other industrial plants. x The removal of [the catalyst] provides new application solutions for the catalyst;
[0040] 3. The bidirectional promoting highly ordered mesoporous WO3 / CeO2 catalyst of this invention is obtained by highly dispersing a low concentration of ammonium metavanadate aqueous solution into a WCe suspension using ultrasonic and vigorous stirring as basic experimental operations, followed by impregnation, drying, and calcination. The preparation method is stable and has broad prospects for industrial application. Attached Figure Description
[0041] Figure 1Figure 'a' shows the conversion trend of nitrogen oxides of the V-bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalysts prepared in Examples 1-3. Figure 1 b is the W prepared in Comparative Example 1. 0.1 Ce 0.9 The conversion trend of nitrogen oxides of CeO2 catalyst prepared in Comparative Example 2, VW / TiO2 catalyst prepared in Comparative Example 3, and V bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst prepared in Example 2 are shown in the figure.
[0042] Figure 2 The V-bidirectional promoting highly ordered mesoporous WO3 / CeO2 catalyst prepared in Example 2 and the W catalyst prepared in Comparative Example 1 are compared. 0.1 Ce 0.9 Evaluation diagram of the water and sulfur resistance properties of highly ordered mesoporous catalysts;
[0043] Figure 3 Image a is a TEM image of the V-bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst prepared in Example 2. Figure 3 b is a HAADF-STEM image of the V-bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst prepared in Example 2. Figure 3 c is the selected area intensity diagram of the V bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst prepared in Example 2;
[0044] Figure 4(a) shows the V bidirectional promoting highly ordered mesoporous WO3 / CeO2 catalyst prepared in Example 2 and the W catalyst prepared in Comparative Example 1. 0.1 Ce 0.9 NH3-TPD of highly ordered mesoporous catalysts;
[0045] Figure 4(b) shows the V bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst prepared in Example 2 and the W catalyst prepared in Comparative Example 1. 0.1 Ce 0.9 In-situ infrared spectra of NH3- adsorption on highly ordered mesoporous catalysts;
[0046] Figure 5(a) shows the V bidirectional promoting highly ordered mesoporous WO3 / CeO2 catalyst prepared in Example 2 and the W catalyst prepared in Comparative Example 1. 0.1 Ce 0.9 H2-TPR diagram;
[0047] Figure 5(b) shows the V bidirectional promoting highly ordered mesoporous WO3 / CeO2 catalyst prepared in Example 2 and the W catalyst prepared in Comparative Example 1. 0.1 Ce 0.9 Ce 3d XPS spectra;
[0048] Figure 5(c) shows the V bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst prepared in Example 2 and the W catalyst prepared in Comparative Example 1. 0.1 Ce 0.9 O1s XPS spectrum. Detailed Implementation
[0049] This invention obtains highly ordered mesoporous CeO2 through hard template reverse substitution; then obtains highly ordered mesoporous WCe catalyst through impregnation; finally, by impregnating V species into the WCe channels again, and calcining, a V bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst is obtained.
[0050] The technical solution of the present invention will be further described below with reference to specific embodiments.
[0051] The main raw materials and their sources of purchase involved in the following examples are as follows:
[0052]
[0053] This application does not impose special requirements on the purity of the raw materials; all required raw materials are of analytical grade and have not undergone further purification.
[0054] The main instruments and models involved in the following embodiments are as follows:
[0055] Instrument Name model Manufacturer Fixed-bed reactor Model FD-2000 Hunan Huasi Instrument Co., Ltd. Electronic analytical balance BSA224S Sartorius, Germany Magnetic stirrer DF-101S Henan Gongyi Yuhua Instrument Equipment Co., Ltd. Electric constant temperature drying oven DH-101 Tianjin Zhonghuan Experimental Electric Furnace Co., Ltd. muffle furnace TM-0217P Tianjin Zhonghuan Experimental Electric Furnace Co., Ltd. Water bath magnetic stirrer ZNCL~GS Tianjin Xingke Technology Co., Ltd. ultrasonic cleaner SB-5200DT Ningbo Xinzhi Biotechnology Co., Ltd.
[0056] To achieve more uniform mass transfer in the solution, vigorous stirring is required when adding tetraethyl orthosilicate (TEOS) and when immersing mesoporous CeO2 in solution B. Ultrasonication is required when mixing the highly ordered mesoporous WCe catalyst with deionized water and when adding ammonium metavanadate aqueous solution dropwise into the WCe suspension.
[0057] The method for preparing the KIT-6 template agent in the following examples includes the following steps:
[0058] S1. Water and hydrochloric acid (HCl concentration of 2 mol / L) are mixed evenly, and then polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer (P123) is added. The mixture is stirred at 350 rpm until homogeneous to obtain the first mixture. The first mixture is then mixed with sodium dodecyl sulfate (SDS) and stirred in a 30°C water bath for 6 hours until homogeneous (to completely dissolve the SDS) to obtain the second mixture. Under stirring conditions (vigorous stirring at 750 rpm), the second mixture is then added... Tetraethyl orthosilicate (TEOS) was added dropwise, and the mixture was stirred at 500 rpm for 24 h to obtain a third mixture. The mixture contained in the following proportions by mass: polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer (P123), sodium dodecyl sulfate (SDS), and tetraethyl orthosilicate (TEOS) were 12:1.38:25.8, and the mixture contained in the following proportions by mass: water, hydrochloric acid, and polyethylene oxide-polypropylene oxide-polyethylene oxide triblock copolymer (P123) were 312:144:12.
[0059] S2, the third mixture is placed in a high-pressure reactor lined with polytetrafluoroethylene and hydrothermally heated at 100°C for 24 hours. After cooling to room temperature, the mixture is filtered to obtain the first precipitate. The first precipitate is washed with deionized water until there is no obvious foam, dried, and ground to obtain a white powder. The white powder is placed in a muffle furnace and calcined at 550°C for 5 hours to obtain KIT-6 template agent. The heating rate to 550°C is 1°C / min.
[0060] KIT-6 template agent was obtained by self-assembly of poly(ethylene oxide-poly(propylene oxide-poly(ethylene oxide)) triblock copolymer (P123) and sodium dodecyl sulfate (SDS) in hydrochloric acid; tetraethyl orthosilicate (TEOS) was added as a silicon source precursor, and P123 and SDS were removed by calcination.
[0061] Examples 1-3
[0062] A method for preparing a V-type bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst includes the following steps:
[0063] Step 1: Cerium nitrate (Ce(NO3)3·6H2O) and deionized water are mixed until homogeneous to obtain solution A. Solution A is mixed with KIT-6 template agent and magnetically stirred at 600 rpm for 24 hours at room temperature (20-30°C). Then, the mixture is stirred at 600 rpm in a 60°C water bath until the solution evaporates to dryness to obtain the first solid. The first solid is ground into powder and placed in a muffle furnace for calcination at 400°C (heating rate to 400°C is 1°C / min) for 4 hours. After cooling to room temperature, it is first dissolved in 50 mL of sodium hydroxide (NaOH) water. The sample was washed twice with liquid to remove the KIT-6 template agent, then washed with deionized water until neutral (pH=7), and dried in an oven at 80℃ for 24h to obtain mesoporous CeO2. The mass ratio of cerium nitrate (Ce(NO3)3·6H2O) to KIT-6 template agent was 3:1.5; the mass ratio of KIT-6 template agent to the volume ratio of deionized water in step 1 was 1.5:30. The mass ratio is in g and the volume ratio is in mL. The concentration of sodium hydroxide in the sodium hydroxide (NaOH) aqueous solution was 2mol / L.
[0064] Step 2: The mesoporous CeO2 is impregnated in solution B. First, it is stirred (vigorously stirred) at 600 rpm for 6 hours at room temperature (20-30°C). Then, it is stirred at 600 rpm in a water bath at 60°C until the solution evaporates to dryness, obtaining a second solid. The second solid is ground into powder and dried in an oven at 80°C for 24 hours. It is then placed in a muffle furnace and calcined at 400°C (heating rate to 400°C is 1°C / min) for 4 hours. After cooling to room temperature, a highly ordered mesoporous WCe catalyst is obtained. Solution B is obtained by mixing ammonium metatungstate hydrate and an aqueous oxalic acid solution (the concentration of oxalic acid in the aqueous oxalic acid solution is Z), stirring at 600 rpm for 30 minutes until homogeneous, obtaining solution B. Based on the molar proportions, the Ce and ammonium metatungstate hydrate ((NH4)2) in the mesoporous CeO2... 10 W 12 O 41 The ratio of W in xH2O is X; the ratio of ammonium metatungstate hydrate to oxalic acid (in oxalic acid aqueous solution) by molar amount is Y. The values of X, Y and Z are shown in Table 1.
[0065] Step 3: Mix the WCe highly ordered mesoporous catalyst with deionized water and sonicate at 40 kHz for 30 min to obtain a WCe suspension. Add 1 mL of ammonium metavanadate (NH4VO3) aqueous solution to the WCe suspension and sonicate at 40 kHz for 30 min. First, stir at 600 rpm for 6 h at room temperature (20-30℃), then stir at 600 rpm in a water bath at 60℃ until the solution evaporates to dryness to obtain a third solid. Grind the third solid into powder, dry it in an oven at 80℃ for 24 h, place it in a muffle furnace, and calcine it at 400℃ (heating rate to 400℃ is 1℃ / min) for 4 h. Cool to room temperature to obtain a V bidirectional promoting highly ordered mesoporous WO3 / CeO2 catalyst (the V bidirectional promoting highly ordered mesoporous WO3 / CeO2 catalysts obtained in Examples 1-3 are V / W respectively). 0.05 Ce 0.95 V / W 0.1 Ce 0.9 and V / W 0.2 Ce 0.8 In the aqueous solution of ammonium metavanadate (NH4VO3), the ratio of ammonium metavanadate to highly ordered mesoporous catalyst WCe is 1:100 by mass, the ratio of the mass fraction of highly ordered mesoporous catalyst WCe to the volume fraction of deionized water in step 3 is 0.3:50, the unit of mass fraction is g, the unit of volume fraction is mL, and the concentration of ammonium metavanadate in the aqueous solution of ammonium metavanadate (NH4VO3) is 2 mg / mL.
[0066] Table 1
[0067] Example X Y Z (unit: mol / L) serial number Example 1 0.95:0.05 1:2 0.0026 <![CDATA[V / W 0.05 This 0.95 ]]> Example 2 0.9:0.1 1:2 0.0055 <![CDATA[V / W 0.1 This 0.9 ]]> Example 3 0.8:0.2 1:2 0.0133 <![CDATA[V / W 0.2 This 0.8 ]]>
[0068] Comparative Example 1
[0069] A WCe catalyst (W 0.1 Ce 0.9 The WCe highly ordered mesoporous catalyst prepared in Example 2 is shown.
[0070] Comparative Example 2
[0071] A CeO2 catalyst (CeO2) is the mesoporous CeO2 prepared in Example 1.
[0072] Comparative Example 3
[0073] A method for preparing a VW / TiO2 catalyst (VW / TiO2) includes the following steps:
[0074] Step 1: Dissolve 0.0318g of ammonium metatungstate hydrate in an oxalic acid aqueous solution (the oxalic acid aqueous solution is obtained by mixing 0.0231g of oxalic acid and 50ml of distilled water), stir for 30min to obtain the first mixed solution. The ratio of ammonium metatungstate hydrate to oxalic acid in the oxalic acid aqueous solution is 1:2 by molar ratio.
[0075] Step 2: Add 1 ml of ammonium metavanadate (NH4VO3) aqueous solution (the mass fraction of ammonium metavanadate in the aqueous solution of ammonium metavanadate (NH4VO3) is 2 mg / mL) to the first mixed solution in Step 1 to obtain the second mixed solution;
[0076] Step 3: Impregnate 0.3g of TiO2 (anatase) support in the second mixed solution, stir at room temperature for 6h, then place in a 60℃ water bath and continue stirring until the solution evaporates to dryness to obtain a solid mixture. Grind the solid mixture and place it in an oven to dry at 100℃ for 12h. Calcinate it in a muffle furnace at 500℃ for 5h (heating rate of 5℃ / min), and cool to room temperature to obtain the VW / TiO2 catalyst.
[0077] To screen for catalysts with optimal catalytic performance, the coordination environment of V was controlled by adjusting the ratio of Ce to W. The V / W bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst (V / W) prepared in Example 1 was tested. 0.05 Ce 0.95 Example 2 prepared a V-bidirectional promoting highly ordered mesoporous WO3 / CeO2 catalyst (V / W 0.1 Ce 0.9 Example 3 prepared a V-bidirectional promoting highly ordered mesoporous WO3 / CeO2 catalyst (V / W 0.2 Ce 0.8 The WCe catalyst obtained in Comparative Example 1 (W 0.1 Ce 0.9 The conversion rates of nitrogen oxides (NOx) of the CeO2 catalyst (CeO2) obtained in Comparative Example 2 and the VW / TiO2 catalyst (VW / TiO2) obtained in Comparative Example 3 were measured at 100-400 °C. The test conditions for NOx conversion were: fixed-bed reaction, 100-400 °C, nitric oxide concentration of 500 ppm, ammonia concentration of 500 ppm, oxygen volume fraction of 5 vol.%, GHSV = 120,000 h⁻¹. -1 The following steps were performed, in which nitrogen was chosen as the balance gas.
[0078] like Figure 1 As shown in Figure a, when the molar ratio of W to Ce is 0.1:0.9, V / W 0.1 Ce 0.9 It exhibits the best denitrification conversion rate (at GHSV = 120,000 h⁻¹).-1 At high gas velocity ratios, a denitrification conversion rate of over 95% is maintained within a temperature range of 225-400℃. (For example...) Figure 1 As shown in b, V / W 0.1 Ce 0.9 The denitrification efficiency is also significantly better than that of the control group.
[0079] Figure 2 V / W 0.1 Ce 0.9 (The V-bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst prepared in Example 2) and W 0.1 Ce 0.9 (W prepared in Comparative Example 1) 0.1 Ce 0.9 Evaluation of the water and sulfur resistance properties of a highly ordered mesoporous catalyst. The evaluation conditions were: 200℃, nitric oxide concentration of 500 ppm, ammonia concentration of 500 ppm, oxygen volume fraction of 5 vol.%, water vapor volume fraction of 5 vol.%, sulfur dioxide concentration of 100 ppm, and GHSV = 120,000 h⁻¹. -1 The following steps were performed, with nitrogen chosen as the balance gas. The V / W ratio was measured at 200°C. 0.1 Ce 0.9 and W 0.1 Ce 0.9 The evaluation of its water and sulfur resistance showed that it performed well at a low temperature of 200℃ and GHSV = 120,000h. -1 At high air speed ratios, V / W 0.1 Ce 0.9 Its water and sulfur resistance is significantly better than W. 0.1 Ce 0.9 .
[0080] Figure 3 Image a is a TEM image of the V-bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst prepared in Example 2. Figure 3 b is a HAADF-STEM image of the V-bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst prepared in Example 2. Figure 3 c is the selected area intensity map of the V bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst prepared in Example 2. Figure 3 a indicates V / W 0.1 Ce 0.9 It exhibits a highly ordered mesoporous structure. Meanwhile, Figure 3 b further analyzed V / W 0.1 Ce 0.9 The exposed crystal facet, with clearly visible individual V dark spots, confirms the high dispersion of the V species. Figure 3c shows that V replaces the Ce site, forming VO-Ce and VOW structures.
[0081] Figure 4(a) shows the V bidirectional promoting highly ordered mesoporous WO3 / CeO2 catalyst prepared in Example 2 and the W catalyst prepared in Comparative Example 1. 0.1 Ce 0.9 Figure 4(b) shows the NH3-TPD of highly ordered mesoporous catalysts, with V bidirectional promotion of highly ordered mesoporous WO3 / CeO2 catalyst prepared in Example 2 and the WO3 / CeO2 catalyst prepared in Comparative Example 1. 0.1 Ce 0.9 In-situ infrared spectrum of NH3- adsorption on a highly ordered mesoporous catalyst. The V / W ratio can be seen from Figure 4(a). 0.1 Ce 0.9 Compared to W 0.1 Ce 0.9 The peaks representing the physical adsorption of -NH3 and B-NH3, located in the 50-200℃ range, are closer to the low-temperature region, indicating that the V / W ratio is lower in the low-temperature range. 0.1 Ce 0.9 W 0.1 Ce 0.9 It is more effective at adsorbing NH3; for the peak at 200-600℃ attributed to L-NH3, V / W 0.1 Ce 0.9 W 0.1 Ce 0.9 The performance is more pronounced, indicating V / W 0.1 Ce 0.9 There are species with stronger Lewis acids. Figure 4(b) further shows W 0.1 Ce 0.9 and V / W 0.1 Ce 0.9 Both Brønsted acid and Lewis acid are present on the surface.
[0082] Figure 5(a) shows the V bidirectional promoting highly ordered mesoporous WO3 / CeO2 catalyst prepared in Example 2 and the W catalyst prepared in Comparative Example 1. 0.1 Ce 0.9 The H2-TPR diagrams; Figure 5(b) shows the V bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst prepared in Example 2 and the W catalyst prepared in Comparative Example 1. 0.1 Ce 0.9 The Ce 3d XPS spectra; Figure 5(c) shows the V bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst prepared in Example 2 and the W catalyst prepared in Comparative Example 1. 0.1 Ce 0.9 O1s XPS spectra. W was determined by hydrogen temperature-programmed desorption. 0.1 Ce 0.9 and V / W 0.1 Ce0.9 The redox ability. As shown in Figure 5(a), V / W 0.1 Ce 0.9 Its redox properties are significantly better than W 0.1 Ce 0.9 As shown in Figure 5(b), V / W 0.1 Ce 0.9 Ce on the surface 3+ The concentration (27.14%) was higher than that of W. 0.1 Ce 0.9 (13.75%) is much higher. As shown in Figure 5(c), V / W 0.1 Ce 0.9 The concentration of surface-adsorbed oxygen (59.18%) was also significantly higher than that of W. 0.1 Ce 0.9 (51.75%). This indicates that the introduction of trace amounts of V greatly enhances the V / W ratio. 0.1 Ce 0.9 Its redox ability.
[0083] The present invention has been described above by way of example. It should be noted that any simple modifications, alterations or other equivalent substitutions that can be made by those skilled in the art without creative effort without departing from the core of the present invention fall within the protection scope of the present invention.
Claims
1. A V-bidirectional promoting highly ordered mesoporous WO3 / CeO2 catalyst, characterized in that, V substitutes for Ce sites, forming VO-Ce and VOW structures and enhancing the surface acidity and redox properties of the V-bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst. The preparation method of the V-bidirectionally promoted highly ordered mesoporous WO3 / CeO2 catalyst includes the following steps: Step 1: Mix cerium salt and water until homogeneous to obtain solution A. Mix solution A with KIT-6 template agent and stir until the solution evaporates to dryness to obtain a first solid. Grind the first solid into powder, calcine at 400~500 ℃ for 4~6 h, cool to room temperature, wash, and dry to obtain mesoporous CeO2. The ratio of cerium salt to KIT-6 template agent by mass is (3~4.5):1.
5. Step 2: Mix mesoporous CeO2 and solution B, stir until the solution evaporates to dryness to obtain a second solid, grind the second solid into powder, dry it, calcine it at 400~500 ℃ for 4~6 h, and cool it to room temperature to obtain a highly ordered mesoporous WCe catalyst. In this case, solution B is a mixture of ammonium metatungstate hydrate, oxalic acid and water. By molar amount, the ratio of Ce in the mesoporous CeO2 to W in the ammonium metatungstate hydrate is 0.9:0.1, and by molar amount, the ratio of ammonium metatungstate hydrate to oxalic acid is 1:(1~3). Step 3: Mix the WCe highly ordered mesoporous catalyst with water, sonicate to obtain a WCe suspension, add an ammonium metavanadate aqueous solution dropwise to the WCe suspension, sonicate, stir until the solution evaporates to dryness to obtain a third solid, grind the third solid into powder, dry it, calcine it at 400~500 ℃ for 4~6 h, and cool it to room temperature to obtain a V bidirectional promoting highly ordered mesoporous WO3 / CeO2 catalyst, wherein, by mass parts, the ratio of ammonium metavanadate to the WCe highly ordered mesoporous catalyst in the ammonium metavanadate aqueous solution is 1:
100.
2. The V-bidirectional promoting highly ordered mesoporous WO3 / CeO2 catalyst according to claim 1, characterized in that, In step 2, the method for obtaining solution B is as follows: ammonium metatungstate hydrate and oxalic acid aqueous solution are mixed and stirred for 30-60 min until homogeneous to obtain solution B, wherein the stirring speed is 500-700 rpm.
3. The V-bidirectional promoting highly ordered mesoporous WO3 / CeO2 catalyst according to claim 1, characterized in that, In step 1, the ratio of the mass fraction of the KIT-6 template agent to the volume fraction of water is 1.5:(30~50), where the mass fraction is in g and the volume fraction is in mL.
4. The V-bidirectional promoting highly ordered mesoporous WO3 / CeO2 catalyst according to claim 1, characterized in that, In step 3, the ratio of the mass fraction of the WCe highly ordered mesoporous catalyst to the volume fraction of water in step 3 is 0.3:(30~50), where the mass fraction is in g and the volume fraction is in mL.
5. The V-bidirectional promoting highly ordered mesoporous WO3 / CeO2 catalyst according to claim 1, characterized in that, In step 3, the concentration of ammonium metavanadate in the aqueous solution is 1~3 mg / mL.
6. The V-bidirectional promoting highly ordered mesoporous WO3 / CeO2 catalyst according to claim 1, characterized in that, In step 1, the washing process involves first washing with an aqueous sodium hydroxide solution to remove the KIT-6 template agent, and then washing with water until neutral. The concentration of sodium hydroxide in the aqueous sodium hydroxide solution is 1.8~3 mol / L.
7. The V-bidirectional promoting highly ordered mesoporous WO3 / CeO2 catalyst according to claim 1, characterized in that, In step 3, the ultrasound duration is 30 to 60 minutes and the ultrasound frequency is 30 to 50 kHz.
8. The V-bidirectional promoting highly ordered mesoporous WO3 / CeO2 catalyst according to claim 1, characterized in that, In steps 1 to 3, the heating rate to 400 to 500 °C is 0.5 to 1 °C / min.
9. The application of the V-bidirectional promoting highly ordered mesoporous WO3 / CeO2 catalyst as described in claim 1 in the removal of nitrogen oxides.
Citation Information
Patent Citations
Medium-low-temperature denitration catalyst with mesoporous cerium oxide as carrier and preparation method
CN109046324A
Cerium oxide for detecting hydrogen peroxide having a mesoporous structure, a method for producing the same, and a biosensor for detecting hydrogen peroxide comprising the same
KR102126781B1