A method for manufacturing a large size prepreg mould press panel
By measuring the flatness deviation of the upper and lower pressure plates of the press in sections, determining the compensation coefficient and process clearance, and optimizing the molding process parameters, the problems of local color difference, delamination and high porosity in the production of large-size plates were solved, and the product quality was improved.
Patent Information
- Application Number
- CN202410594099.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-14
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-05-14
AI Technical Summary
In the process of large-size compression molding, the flatness deviation of the upper and lower plates of the press leads to problems such as excessive local color difference, delamination, high porosity and uneven thickness during the production of the sheet material.
By measuring the flatness deviation of the upper and lower pressure plates of the press in sections, the compensation coefficient and process clearance are determined. Combined with the thickness and thermal expansion characteristics of silicone rubber, the flatness deviation of the pressure plates is compensated, and the molding process parameters are optimized to improve the quality of the sheet.
It effectively solves the problems of local color difference, delamination and high porosity in large-size boards, and improves the yield and quality stability of products.
Smart Images

Figure CN118404832B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of composite material molding technology, specifically relating to a method for manufacturing large-size prepreg molded sheets. Background Technology
[0002] Compression molding is a common and widely used method in the production of composite materials. It has advantages such as high dimensional accuracy, good repeatability, high efficiency, ease of specialization and automation, suitability for mass production, and low cost.
[0003] When the press is large, the flatness of its upper and lower hot platens can only be guaranteed within a certain reasonable range. Furthermore, the press will inevitably develop flatness issues over prolonged use. For example, some manufacturers specify that a flatness of less than 0.3-0.4mm for the upper and lower platens of a 3m long and 2m wide press is considered acceptable. However, this can lead to quality problems such as excessive local color differences, delamination, high porosity, and uneven thickness when producing large-sized sheets.
[0004] Therefore, there is an urgent need for a manufacturing method for large-size prepreg molded sheets to solve quality problems such as excessive local color difference, delamination, high porosity, and uneven thickness that occur when producing large-size sheets.
[0005] The information disclosed in this background section is intended only to enhance the understanding of the overall background of the invention and should not be construed as an admission or in any way implying that the information constitutes prior art known to those skilled in the art. Summary of the Invention
[0006] The purpose of this invention is to provide a method for manufacturing large-size prepreg molded sheets, which can solve the problems mentioned in the background art.
[0007] To achieve the above objectives, a specific embodiment of the present invention provides the following technical solution: A method for manufacturing large-size prepreg molded sheets includes the following steps: S1, determining the maximum flatness deviation of the upper and lower plates of the press; dividing the upper and lower plates of the press into different areas, and testing the maximum flatness deviation of different areas of the upper and lower plates respectively. S2, determining the compensation coefficient n: determining the compensation coefficient n based on the ratio of the flatness deviations of corresponding areas of the upper and lower plates of the press; S3, determining the process clearance: determining the molding process clearance based on process parameters; S4, laying and curing: sequentially laying steel plate, prepreg, steel plate and silicone rubber on the surface of the lower press, setting the temperature of the upper and lower plates of the press, heating time, and process clearance, and heating and curing; after curing, removing the auxiliary materials to obtain the product.
[0008] In one or more embodiments of the present invention, the specific steps for determining the maximum flatness deviation of the upper and lower pressure plates of the press in step S1 are as follows: The length of the long side of the press plate is denoted as m, and the length of the short side is denoted as M. The long side m and the short side M of the press plate are divided into equal parts, denoted as p and q respectively. The corresponding dividing points are connected to form a certain number of grids, and each grid corresponds to a region. The maximum flatness deviation of each region of the upper and lower press plates is tested. p and q are determined according to the following formula:
[0009] In one or more embodiments of the present invention, the number of partitions of the upper and lower pressure plates of the press is consistent with the partitioning rules, and the upper and lower pressure plates correspond one-to-one.
[0010] In one or more embodiments of the present invention, in step S2, the compensation coefficient n is determined according to the following formula:
[0011] T n T m These are the flatness deviation values of the corresponding areas of the upper and lower pressure plates of the press, respectively, and T n Greater than T m .
[0012] In one or more embodiments of the present invention, the process parameters include prepreg layup, bulk modulus of silicone rubber, molding expansion pressure, coefficient of volume expansion, room temperature, resin gelation temperature, and silicone rubber thickness.
[0013] In one or more embodiments of the present invention, the process gap is determined according to the following formula:
[0014] In one or more embodiments of the present invention, T gel T1 is the resin gelation temperature, and P is the room temperature. ge l represents the resin gelation temperature, which is equal to T. gel The thermal expansion pressure at time T, K is the bulk modulus of elasticity, V is the volume loss due to thermal expansion of silicone rubber, and V is the gel temperature equal to T. gel V1 is the volume of silicone rubber at temperature T1, is the volume expansion coefficient of silicone rubber, L is the process gap, T is the maximum flatness deviation of the upper and lower pressure plates of the press, S is the prepreg laying area, n is the compensation coefficient, and H is the thickness of silicone rubber.
[0015] In one or more embodiments of the present invention, the length and width of the silicone rubber are equal to the length and width of the prepreg layer.
[0016] In one or more embodiments of the present invention, the thickness H of the silicone rubber is 5~20mm.
[0017] In one or more embodiments of the present invention, each of the grids is the same size.
[0018] Compared with the prior art, the present invention provides a method for manufacturing large-size prepreg molding sheets by establishing partitions on the upper and lower plates of the press and measuring and analyzing the flatness of each partition. Combined with the characteristics of the specific product molding process, the thickness of the silicone rubber and the process gap are determined. The thermal expansion of the silicone rubber provides pressure to compensate for quality problems such as excessive local color difference, delamination, high porosity and uneven thickness caused by the flatness deviation of the press plates, thereby improving the yield and product quality stability. Attached Figure Description
[0019] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0020] Figure 1 This is a flowchart illustrating a method for manufacturing large-size prepreg molded sheets according to an embodiment of the present invention. Figure 2 This is a schematic diagram of the partitioning of the upper pressure plate of the press in one embodiment of the present invention; Figure 3 This is a schematic diagram of the partitioning of the lower pressure plate of the press in one embodiment of the present invention; Figure 4 This refers to the flatness data of the upper pressure plate of the press in one embodiment of the present invention; Figure 5 This refers to the flatness data of the lower pressure plate of the press in one embodiment of the present invention; Figure 6 This is the ratio of the flatness deviations of the corresponding areas of the upper and lower pressure plates of the press in one embodiment of the present invention; Figure 7 This is a schematic diagram of a press molding process in one embodiment of the present invention; Figure 8 This is a quality comparison diagram of the embodiments and comparative examples in this invention. Detailed Implementation
[0021] To enable those skilled in the art to better understand the technical solutions of this invention, the technical solutions of the embodiments of this invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this invention, and not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of this invention.
[0022] like Figure 1 As shown, in one embodiment of the present invention, a method for manufacturing large-size prepreg molded sheets involves determining the maximum flatness deviation of the upper and lower press plates of the press, dividing the upper and lower press plates of the press into different regions, and testing the maximum flatness deviation of different regions of the upper and lower press plates respectively.
[0023] like Figure 2 As shown, the dimensions of the upper platen of the press are length m and width M. The long side m and short side M of the upper platen are each divided into equal lengths, denoted as p and q, respectively, where p is 0.3m and q is 0.28m. The corresponding dividing points are connected to form a certain number of grids, each grid corresponding to a region. The values of p and q can be determined using the following formula:
[0024] Ultimately, p was determined to be 300mm and q to be 280mm. The values of p and q determined the size of the grid, which should ideally be between 100 and 300. A grid that is too large cannot accurately assess the flatness of the press platen, thus making it impossible to accurately determine the thickness of the silicone rubber and achieve effective expansion pressure compensation. A grid that is too small significantly increases the workload of actual operation. Figure 2 As shown, the upper platen of the press is divided into 100 grid intervals, numbered from 1 to 100.
[0025] like Figure 3 As shown, the number and rules of the partitions of the lower platen of the press are the same as those of the upper platen of the press, and the upper and lower plates correspond one-to-one, divided into 100 grid intervals, numbered from 1-1 to 100-1.
[0026] like Figures 4-5 As shown, the flatness of 100 grid zones on the upper and lower pressure plates of the press was measured. The silicone rubber thickness compensation coefficient n was determined based on the ratio of the flatness deviations of corresponding areas on the upper and lower pressure plates. The compensation coefficient n can be determined using the following formula:
[0027] refer to Figure 4 , Figure 5 and Figure 6 As shown, the maximum flatness deviation of the upper pressure plate grid section 25 is 136 μm, while the corresponding maximum flatness deviation of the lower pressure plate grid section 25-1 is 173 μm. The flatness deviation of the upper pressure plate is smaller than that of the lower pressure plate. n It is 173 μm, T m It is 136μm, T n With T mThe previous ratio was 1.27. The maximum flatness deviation of the upper pressure plate grid section 55 was 389 μm, while the corresponding maximum flatness deviation of the lower pressure plate grid section 25-1 was 197 μm. The flatness deviation of the upper pressure plate was greater than that of the lower pressure plate. T n The value is 389 μm, Tm is 197 μm, and T n With T m The previous ratio was 1.27. After final calculation, the minimum ratio was 1.01. The compensation coefficient was determined to be 1.5 according to the formula. The corresponding flatness deviation is 187μm for the upper pressure plate grid number 43 and 186μm for the lower pressure plate grid number 43-1.
[0028] Determine the size of the silicone rubber. Based on the prepreg layup, the bulk modulus of elasticity of the silicone rubber, the expansion pressure required for curing the prepreg, the volume expansion coefficient of the silicone rubber, room temperature, and resin gelation temperature, determine the length, width, and thickness of the silicone rubber for the upper and lower pressure plates. The length and width of the silicone rubber should be consistent with the prepreg layup dimensions.
[0029] Installation and curing, such as Figure 7 As shown, from bottom to top, the components are: lower press platen, steel plate, prepreg, steel plate, silicone rubber, and upper press platen. The steel platen, prepreg, and silicone rubber are sequentially laid on the surface of the lower press. The temperatures, heating times, and process intervals of the upper and lower press plates are set, and the mixture is heated and cured. After curing, the auxiliary materials are removed to obtain the product.
[0030] Generally, the thickness H of the silicone rubber is 5~20mm, and the thickness of the steel plate is 0.3~1mm.
[0031] Example 1: The finished sheet has a length of 2600mm, a width of 2500mm, and a thickness of 0.18mm. The prepreg is unidirectional carbon fiber epoxy resin prepreg with a single layer thickness of 0.06mm and a layup angle of [0 / 90 / 0]. The prepreg has a layup length of 2650mm and a width of 2550mm. The length and width of the silicone rubber are the same as the prepreg layup dimensions. In this embodiment, the room temperature is 22℃. At room temperature, the silicone rubber has a length of 2650mm and a width of 2550mm. The thickness H of the silicone rubber is 12mm, and the steel plate thickness is 0.5mm.
[0032] The process clearance L can be determined according to the following formula:
[0033] Among them, T gel T1 is the resin gelation temperature, P is the room temperature. gel The resin gelation temperature is equal to T. gel The thermal expansion pressure at that time, where K is the bulk modulus of elasticity. V represents the volume loss due to thermal expansion of silicone rubber, where V is the gel temperature equal to T. ge V1 is the free expansion volume of the silicone rubber at temperature T1, where V1 is the volume of the silicone rubber at temperature T1. denoted as the volume expansion coefficient of silicone rubber, L as the process gap, T as the maximum flatness deviation of the upper and lower pressure plates of the press, S as the prepreg laying area, n as the compensation coefficient, and H as the thickness of silicone rubber.
[0034] The bulk modulus K of silicone rubber is 720 MPa, the coefficient of volume expansion is 8.1 × 10⁻⁴ / ℃, the prepreg molding process pressure is 0.4 MPa, and the resin gelation temperature T is... gel The temperature is 130℃, T is the maximum flatness deviation of the 55 grid sections corresponding to the upper pressure plate, which is 0.389mm, and the compensation coefficient n is 1.5. Substituting all parameters into the formula for calculating the process clearance L, L can be obtained. In this example, the value of L obtained is 0.46mm.
[0035] A 0.5mm thick steel plate, carbon fiber epoxy resin prepreg, and 12mm thick silicone rubber are sequentially laid onto the lower press plate. The distance between the upper press plate and the silicone rubber is adjusted to 0.46mm. The temperature and heating time of the upper and lower press plates are set and the material is heated and cured. After curing, the auxiliary materials are removed to obtain the product.
[0036] Example 2: The finished sheet has a length of 2600mm, a width of 2500mm, and a thickness of 0.36mm. The prepreg is unidirectional glass fiber phenolic prepreg with a single layer thickness of 0.12mm and a layup angle of [0 / 90 / 0]. The prepreg has a layup length of 2650mm and a width of 2550mm. The length and width of the silicone rubber are the same as the prepreg layup dimensions. In this embodiment, the room temperature is 22℃. At room temperature, the silicone rubber has a length of 2650mm and a width of 2550mm. The thickness H of the silicone rubber is 14mm, and the steel plate thickness is 0.5mm.
[0037] The bulk modulus K of silicone rubber is 720 MPa, and its coefficient of volume expansion is... The temperature is 8.1 × 10⁻⁴ / ℃, the prepreg molding process pressure is 1.2 MPa, and the resin gelation temperature is T. gel The temperature is 150℃, T is the maximum flatness deviation of the 55 grid sections corresponding to the upper pressure plate, which is 0.389mm, and the compensation coefficient n is 1.5. Substituting all parameters into the formula for calculating the process clearance L, L can be obtained. In this example, the value of L obtained is 0.84mm.
[0038] A 0.5mm thick steel plate, glass fiber phenolic prepreg, and 12mm thick silicone rubber are sequentially laid onto the lower press plate. The distance between the upper press plate and the silicone rubber is adjusted to 0.84mm. The temperature and heating time of the upper and lower press plates are set and the material is heated and cured. After curing, the auxiliary materials are removed to obtain the product.
[0039] Example 3: The finished sheet has a length of 2600mm, a width of 2500mm, and a thickness of 0.45mm. The prepreg is made of glass fiber plain weave phenolic prepreg with a single layer thickness of 0.15mm. Three layers are laid, with the prepreg layer measuring 2650mm in length and 2550mm in width. The length and width of the silicone rubber are consistent with the dimensions of the prepreg layer. In this embodiment, the room temperature is 22℃. At room temperature, the silicone rubber is 2650mm in length and 2550mm in width, the thickness H of the silicone rubber is 15mm, and the steel plate thickness is 0.6mm.
[0040] In this embodiment, the bulk modulus K of the silicone rubber is 720 MPa, and the coefficient of volume expansion is... The temperature is 8.1 × 10⁻⁴ / ℃, the prepreg molding process pressure is 1.4 MPa, and the resin gelation temperature is T. ge l is 150℃, T is the maximum flatness deviation of the upper pressure plate corresponding to grid 55 partition is 0.389mm, and the compensation coefficient n is 1.5. Substituting all parameters into formula (1-3) can calculate L. In this example, the calculated value of L is 0.94mm.
[0041] A 0.6mm thick steel plate, a glass fiber plain weave phenolic prepreg, a 0.6mm thick steel plate, and a 15mm thick silicone rubber are sequentially laid onto the lower press plate. The distance between the upper press plate and the silicone rubber is adjusted to 0.94mm. The temperature and heating time of the upper and lower press plates are set and the material is heated and cured. After curing, the auxiliary materials are removed to obtain the product.
[0042] Comparative Example 1: The finished sheet has a length of 2600mm, a width of 2500mm, and a thickness of 0.18mm. The prepreg is unidirectional carbon fiber epoxy resin prepreg with a single layer thickness of 0.06mm and a layup angle of [0 / 90 / 0]. The prepreg is laid in a length of 2650mm and a width of 2550mm at a room temperature of 22℃. The steel plate is 0.5mm thick.
[0043] A 0.5mm thick steel plate, carbon fiber epoxy resin prepreg, and another 0.5mm thick steel plate are sequentially laid onto the lower press plate. The temperature, heating, and pressurization time of the upper and lower press plates are set, and the plates are heated and cured. The curing pressure is the same as that of Comparative Example 1. After curing, the auxiliary materials are removed to obtain the product.
[0044] Comparative Example 2: The finished board has a length of 2600mm, a width of 2500mm, and a thickness of 0.36mm. The prepreg is unidirectional glass fiber phenolic prepreg with a single layer thickness of 0.12mm and a layup angle of [0 / 90 / 0]. The prepreg is laid in a length of 2650mm and a width of 2550mm at an ambient temperature of 22℃. The steel plate is 0.5mm thick.
[0045] A 0.5mm thick steel plate, glass fiber phenolic prepreg, and another 0.5mm thick steel plate are sequentially laid onto the lower press plate. The temperature, heating, and pressurization time of the upper and lower press plates are set, and the product is heated and cured. The curing pressure is the same as that of Comparative Example 2. After curing, the auxiliary materials are removed to obtain the product.
[0046] Comparative Example 3: The finished board dimensions are 2600mm long, 2500mm wide, and 0.45mm thick. The prepreg is made of glass fiber plain weave phenolic prepreg with a single layer thickness of 0.15mm. Three layers are laid, with the prepreg laid in a length of 2650mm and a width of 2550mm. The room temperature is 22℃, and the steel plate thickness is 0.6mm.
[0047] A 0.6mm thick steel plate, a glass fiber plain weave phenolic prepreg, and a 0.6mm thick steel plate are sequentially laid onto the lower press plate. The temperature, heating and pressurization time of the upper and lower press plates are set and the product is heated and cured. The curing pressure is the same as that of Comparative Example 3. After curing, the auxiliary materials are removed to obtain the product.
[0048] The quality of the products from Examples 1-3 and Comparative Examples 1-3 of this invention was compared, and the results are as follows: Figure 8 As shown, through observation and testing of the composite material sheets in the examples and comparative examples, it was found that for prepreg molding with different resin systems, curing pressures, and layup thicknesses, this invention effectively solves the quality problems of excessive local color difference, delamination, high porosity, and uneven thickness in the molding of large-size sheets. Table 1 above shows that the molding pressure required for Comparative Examples 1, 2, and 3 gradually increases. Due to differences in the flatness of the press plates, significant color differences exist in the comparative examples. In Comparative Examples 2 and 3, the prepreg is phenolic resin, requiring even higher curing pressures. Simultaneously, gas release occurs during curing, leading to local delamination where the flatness of the upper and lower press plates differs. This invention, by improving the traditional composite material sheet molding process, effectively solves the quality problems encountered in actual production processes in Examples 1-3.
[0049] As can be seen from the above technical solutions, the present invention has the following beneficial effects: by establishing partitions on the upper and lower pressure plates of the press and measuring and analyzing the flatness of each partition, and combining the characteristics of the specific product molding process, the thickness of the silicone rubber and the process gap are determined. The thermal expansion of the silicone rubber provides pressure to compensate for quality problems such as excessive local color difference, delamination, high porosity and uneven thickness caused by the flatness deviation of the press plate, thereby improving the yield and product quality stability.
[0050] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No reference numerals in the claims should be construed as limiting the scope of the claims.
[0051] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
Claims
1. A method for manufacturing large-size prepreg molded sheets, characterized in that, Includes the following steps: S1. Determine the maximum flatness deviation of the upper and lower pressure plates of the press; The upper and lower pressure plates of the press are divided into different areas, and the maximum flatness deviation of different areas of the upper and lower pressure plates is tested respectively. S2. Determine the compensation coefficient n: The compensation coefficient n is determined based on the ratio of the flatness deviations of corresponding areas of the upper and lower pressure plates of the press; S3. Determine the process clearance: Determine the gap in the compression molding process based on the process parameters; S4. Laying and curing: Steel plates, prepreg, and silicone rubber are sequentially laid on the surface of the press. The temperature of the upper and lower plates, the heating time, and the process gap are set and then heated and cured. After curing, the auxiliary materials are removed to obtain the product. The process parameters include prepreg layup, bulk modulus of silicone rubber, molding expansion pressure, coefficient of volume expansion, room temperature, resin gelation temperature, and silicone rubber thickness. The process clearance is determined according to the following formula: Among them, T gel T1 is the resin gelation temperature, and T2 is the room temperature. P gel The resin gelation temperature is equal to T. gel The thermal expansion pressure at that time, where K is the bulk modulus of elasticity. V represents the volume loss due to thermal expansion of silicone rubber, where V is the gel temperature equal to T. gel V1 is the volume of silicone rubber at temperature T1, representing the volume of silicone rubber under free expansion. denoted as the volume expansion coefficient of silicone rubber, L as the process gap, T as the maximum flatness deviation of the upper and lower pressure plates of the press, S as the prepreg laying area, n as the compensation coefficient, and H as the thickness of silicone rubber.
2. The method for manufacturing large-size prepreg molded sheets according to claim 1, characterized in that, In step S1, the specific steps for determining the maximum flatness deviation of the upper and lower pressure plates of the press are as follows: The length of the long side of the press plate is denoted as m, and the length of the short side is denoted as M. The long side m and the short side M of the press plate are divided into equal parts, denoted as p and q respectively. The corresponding dividing points are connected to form a certain number of grids, and each grid corresponds to a region. The maximum flatness deviation of each region of the upper and lower press plates is tested. p and q are determined according to the following formula: .
3. The method for manufacturing large-size prepreg molded sheets according to claim 2, characterized in that, The number of partitions on the upper and lower pressure plates of the press is consistent with the partitioning rules, and the upper and lower pressure plates correspond one-to-one.
4. The method for manufacturing large-size prepreg molded sheets according to claim 1, characterized in that, In step S2, the compensation coefficient n is determined according to the following formula: T n、 T m These are the flatness deviation values of the corresponding areas of the upper and lower pressure plates of the press, respectively, and T n Greater than T m .
5. The method for manufacturing large-size prepreg molded sheets according to claim 1, characterized in that, The length and width of the silicone rubber are equal to the length and width of the prepreg layer.
6. A method for manufacturing large-size prepreg molded sheets according to claim 1 or 5, characterized in that, The thickness H of the silicone rubber is 5~20mm.
7. The method for manufacturing large-size prepreg molded sheets according to claim 1, characterized in that, In step S4, the thickness of the steel plate being laid is 0.3~1mm.
8. A method for manufacturing large-size prepreg molded sheets according to claim 2, characterized in that, Each of the grids is the same size.
Citation Information
Patent Citations
Method for pressurizing and molding composite part by using thermal expansion of silicone rubber
CN101890807A