A method for synthesizing porous carbon by a template method combined with a foaming method and porous carbon
By combining NaCl powder templates and NaHCO₃ powder foaming agents, the problems of unstable preparation process and uneven pore size of sodium bicarbonate foaming agents were solved, realizing a uniform pore structure and high porosity of porous carbon materials, simplifying the preparation process and reducing costs.
Patent Information
- Application Number
- CN202410542288.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-30
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-04-30
AI Technical Summary
In existing technologies, when sodium bicarbonate is used as a foaming agent, the preparation process is unstable and the pore size is uneven, making it difficult to meet the functional requirements of porous materials.
Using NaCl powder as a template and NaHCO₃ powder as a foaming agent, porous carbon is synthesized through a template method and a foaming method. This controls the pore structure, avoids cracks caused by differences in thermal expansion coefficients, and simplifies the preparation process.
This method produces porous carbon materials with uniform pore size and high porosity, which simplifies the preparation process, reduces costs, and improves the intrinsic strength and thermal insulation effect of the materials.
Smart Images

Figure CN118419902B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of porous material preparation technology, specifically relating to a method for synthesizing porous carbon using a template method combined with a foaming method, and the porous carbon itself. Background Technology
[0002] With the rapid development of modern science and technology, newer and higher requirements have been placed on structural and functional materials. Porous carbon materials have been widely studied and applied due to their excellent properties such as high specific surface area, high porosity, and good controllability. Carbon foam consists of two parts: pores and solids. Its pore structure and size are affected by raw materials, preparation methods, and process conditions. In recent years, with the continuous deepening of research on carbon foam and the continuous expansion of its application fields, the main research directions of carbon foam materials have focused on the selection of inexpensive, readily available, and environmentally friendly precursor materials, the modification and alteration of precursors, the development of new preparation methods, and the optimization of existing preparation processes, in order to improve the internal microstructure of carbon foam and thus adjust the thermal, mechanical, and electrical properties of the material. The application fields of carbon foam have also gradually expanded to heat exchangers, aerospace, supercapacitors, and catalyst supports.
[0003] Currently, the main carbon source precursors selected include phenolic resin, polyvinyl chloride (PVC), polyacrylonitrile (PAN), and mesophase pitch. Preparation processes mainly include template method, foaming method, polymer pyrolysis method, and sol-gel method. Among these, phenolic resin is a good precursor and carbon source for preparing carbon foam due to its high carbon content, low toxic gas production during pyrolysis, good flame retardancy, and ease of control. Sodium bicarbonate is a highly efficient and non-toxic foaming agent used in the foaming of resins, gypsum, rubber, etc. It decomposes to produce gas under certain temperature conditions. By controlling its content and foaming temperature, the pore structure of the precursor can be controlled.
[0004] Reference 1, "Feng Na, Wang Weiting, Chang Suqin, et al. Structure and properties of microporous chlorosulfonated polyethylene rubber (CSM) materials with different open and closed pore morphologies prepared by compression molding foaming technology with NaHCO3 as a synergistic foaming agent, shows that with the increase of NaHCO3 content, the average pore diameter increases, the pore wall becomes thinner, and the open porosity increases. However, sodium bicarbonate has a low decomposition temperature and a wide decomposition temperature range, which is not conducive to the formation of uniform and fine pores during the foaming process of materials. It is only suitable for foaming some materials with low crystallization temperature, which limits its application in porous materials and cannot meet the functionalization requirements of foamed materials.
[0005] Reference 2, "Wilson P, Vijayan S, Prabhakaran K. Low-density microcellular carbon foams from sucrose by NaCl particle templating using glycerol as aplasticizing additive[J]. Materials & Design, 2018, 139: 25-35," uses NaCl as a template. A NaCl powder paste is obtained from molten sucrose using a thermal mixing method, followed by heat treatment at 160°C in a steel mold. Subsequently, the sample is pyrolyzed and washed with water to obtain carbon foam. However, its pore size is mainly distributed in the range of 3-9 μm, which is relatively uniform and its structure and properties require further improvement.
[0006] To address the aforementioned issues, this invention utilizes environmentally friendly and readily available NaCl powder as a template. After curing, deionized water can be used to pre-leach the NaCl from the organic precursor before heat treatment (the heat treatment temperature must be higher than the melting points of NaCl and NaHCO3). This avoids the generation and propagation of internal cracks due to the significant difference in thermal expansion coefficients between NaCl particles and phenolic foam during heat treatment, which would affect its pore structure and performance. Simultaneously, NaHCO3 powder is selected as a foaming agent to enrich its pore structure, further reducing its thermal conductivity and achieving excellent thermal insulation. Through simple mechanical stirring, a carbon foam material with uniform distribution and adjustable pore size is prepared, greatly simplifying the preparation process, shortening the preparation cycle, and reducing manufacturing costs. Summary of the Invention
[0007] This invention provides a method for synthesizing porous carbon using a template method combined with a foaming method, and the porous carbon itself, which solves the problems of unstable process and uneven pore size in the current preparation using sodium bicarbonate as a foaming agent.
[0008] To achieve the above objectives, the technical solution adopted by the present invention is: a method for synthesizing porous carbon using a template method combined with a foaming method, comprising the following steps:
[0009] A uniform mixed solution is obtained by mixing carbon-rich resin with water-soluble salt template, foaming agent, surfactant, and curing agent in a set ratio.
[0010] The mixed solution is poured into a mold to foam and solidify. After demolding, the organic precursor foam is obtained.
[0011] The organic precursor foam was soaked in water to remove water-soluble salt templates and then dried to obtain a porous carbon precursor.
[0012] Then, by heating and carbonizing in an inert atmosphere, a porous carbon foam material with a porosity of up to about 80% and uniform distribution can be obtained.
[0013] Furthermore, the carbon-rich resin is a phenolic resin, an epoxy resin, or an organosilicon resin.
[0014] Furthermore, the water-soluble salt template is NaCl, the foaming agent is NaHCO3 powder, and the NaHCO3 powder needs to be ground before being added; the curing agent is powder particles, and the curing agent powder particles need to be ground before being added; the surfactant is Tween-80 or Span-80.
[0015] Furthermore, the mass ratio of the carbon-rich resin, water-soluble salt template, foaming agent, surfactant, and curing agent is 10-20:1-20:1-3:1-5:0.5-5.
[0016] Furthermore, curing is carried out under heating conditions, using a vacuum drying oven, forced-air drying oven, water bath, oil bath, or heating platform to cure and foam the precursor solution. The curing temperature is 50-150℃, and the treatment time is at least 48 hours.
[0017] Furthermore, the organic carbon precursor foam after foaming and curing and demolding is soaked in water to drain the template and then dried to obtain the organic precursor foam.
[0018] Furthermore, the inert atmosphere is argon or nitrogen, the carbonization temperature is 650-1000℃, the heating rate is 5℃ / min, and the holding time is 0.5-3h.
[0019] Furthermore, the organic precursor foam can be directly graphitized during heat treatment, or graphitized again after carbonization to obtain porous graphite materials.
[0020] Furthermore, porous carbon of a set size or shape can be obtained by designing molds, cutting and polishing organic precursor foam to obtain porous carbon of a set size or shape, or cutting and polishing carbonized products to obtain porous carbon of a set size or shape. Similarly, porous graphite of a set size or shape can be obtained by cutting and polishing graphite products after graphitization treatment.
[0021] A porous carbon, prepared by the above-mentioned template method combined with the foaming method, has a porosity of not less than 60% and a pore size of 100-500 μm.
[0022] Compared with existing technologies, this invention has at least the following advantages: This invention proposes a method for preparing porous carbon materials, combining the sodium bicarbonate foaming method with a salt template method that can produce uniform and easily controllable pore structures. On the one hand, it avoids the damage to the precursor and pore structure caused by acids and alkalis during template removal, and the hindered shrinkage during heat treatment due to the different thermal expansion coefficients of the template and precursor resin, which can lead to porous structure damage or cracking. On the other hand, it reduces the amount of foaming agent used, while the template particles stabilize the foam and enrich the pore structure. By controlling the ratio of foaming agent, template, and carbon source, porous carbon materials with a pore size distribution ranging from 100μm to 500μm can be obtained, and the pores are in surface contact with resin and carbon as the bonding area, significantly improving their intrinsic strength. The porous carbon materials prepared by this method have uniform pores, shorten the preparation cycle, simplify the preparation process, reduce preparation costs, and the entire preparation process is environmentally friendly and safe, making it suitable for large-scale production.
[0023] Thoroughly grinding the NaHCO3 powder ensures uniformity and prevents incomplete dissolution and agglomeration of the foaming agent, which can lead to structural defects. Attached Figure Description
[0024] Figure 1 Macroscopic photographs of the foam precursor prepared for the mold before and after carbonization.
[0025] Figure 2 This is a scanned electron image of carbon foam after carbonization at 900℃.
[0026] Figure 3 The image shows the XRD pattern of the carbon foam sample after carbonization at 900℃. It can be seen that in addition to resin carbon, the carbonized sample also contains a small amount of sodium chloride. This is because some sodium chloride particles were sealed by the resin during immersion in water after curing, preventing water from dissolving them. Some of these particles also partially melted and evaporated during carbonization, depositing on the sample surface. This can be removed by subsequent ultrasonic or immersion in water. Figure 4 Macroscopic photographs of samples prepared for molds of different shapes before and after heat treatment following cutting and polishing.
[0027] Figure 5 Scanning electron microscopy (SEM) image of carbon foam after carbonization at 1000°C with the addition of finer salt particles.
[0028] Figure 6 This is a scanned electron image of carbon foam after graphitization treatment at 2100℃. Detailed Implementation
[0029] To further understand the present invention, the following description is provided in conjunction with embodiments.
[0030] Example 1:
[0031] Sodium bicarbonate powder (foaming agent) and hexamethylenetetramine (curing agent) were ground in advance. 15g of phenolic resin was weighed and poured into a 150mL beaker. 2mL of anhydrous ethanol was added to adjust the viscosity of the phenolic resin. After stirring evenly, 5g of sodium chloride powder and 1.5g of pre-ground sodium bicarbonate were added. The mixture was stirred at room temperature for 30min. 2g of surfactant Tween-80 and 2g of curing agent hexamethylenetetramine were added to the mixed solution. The mixture was stirred at room temperature for 30min until the mixed solution was completely dissolved. The precursor solution was then prepared.
[0032] After the prepared solution has been allowed to stand until it is stable and no longer foams at room temperature, it is poured into a mold and then placed in a drying oven for foaming and curing. The temperature of the drying oven is set to 50°C and left for at least 48 hours to allow it to cure completely.
[0033] After complete curing, demold and soak in warm water to drain the sodium chloride template from the precursor foam. Then place in a drying oven to dry.
[0034] After the phenolic foam was dried, the sample was carbonized by heating it to 900℃ at a rate of 5℃ / min under argon protection and holding it at that temperature for 3 hours to obtain non-graphitized carbon foam. Figure 1 As shown, the prepared carbon foam has a uniform pore structure on a macroscopic scale and no obvious defects.
[0035] Example 2:
[0036] Sodium bicarbonate powder, the foaming agent, was ground in advance. 20g of phenolic resin was weighed and poured into a 150mL beaker. 2mL of anhydrous ethanol was added to adjust the viscosity of the phenolic resin. After stirring evenly, 20g of sodium chloride powder and 3g of pre-ground sodium bicarbonate were added. The mixture was stirred at room temperature for 30min. 5g of surfactant Tween-80 and 5g of NL curing agent were added to the mixed solution. The mixture was stirred at room temperature for 60min until the mixed solution was completely dissolved. The precursor solution was then prepared.
[0037] After the prepared solution has been allowed to stand until it stabilizes and does not foam at room temperature, it is poured into a mold and then placed in a drying oven for foaming and curing. The drying oven temperature is set to 90℃ and left for at least 48 hours to allow it to cure completely.
[0038] After complete curing, demold and soak in warm water to drain the sodium chloride template from the precursor foam. Then place in a drying oven to dry.
[0039] After the phenolic foam was dried, the sample was carbonized by heating it to 650℃ at a rate of 5℃ / min under argon protection and holding it at that temperature for 0.5h to obtain non-graphitized carbon foam. The prepared carbon foam had a uniform pore structure and no obvious defects.
[0040] Example 3:
[0041] Sodium bicarbonate powder, the foaming agent, is ground in advance; 10g of phenolic resin is weighed and poured into a 100mL beaker, 1mL of anhydrous ethanol is added to adjust the viscosity of the phenolic resin, and after stirring evenly, 1g of sodium chloride powder and 1g of pre-ground sodium bicarbonate are added, and stirred at room temperature for 30min; 1g of surfactant Tween-80 and 0.5g of NL curing agent are added to the mixed solution, and stirred at room temperature for 30min until the mixed solution is completely dissolved, and the precursor solution is prepared.
[0042] After the prepared solution has been allowed to stand until it stabilizes and does not foam at room temperature, it is poured into a mold and then placed in a vacuum drying oven for foaming and curing. The temperature of the drying oven is set to 150℃ and left for at least 48 hours to allow it to foam and cure completely.
[0043] After complete curing, demold and soak in warm water to drain the sodium chloride template from the precursor foam. Then place in a drying oven to dry.
[0044] After the phenolic foam is dried, the sample is cut, polished, cleaned, dried again, and then carbonized. Under argon protection, the temperature is raised to 900℃ at a rate of 5℃ / min and held for 3 hours to obtain non-graphitized carbon foam. Figure 4 As shown, the prepared carbon foam has a uniform pore structure on a macroscopic scale and no obvious defects.
[0045] Figure 2 The scanning images show that the non-graphitized porous carbon obtained after carbonization at 900℃ has a smooth pore wall surface without obvious cracks and defects, good connection at the ligament and uniform microstructure, and the pore size is mainly distributed between 200-400μm. The pores are in surface contact with each other with resin carbon as the bonding area.
[0046] The porous carbon material prepared by the method of this invention can float to the surface in an aqueous solution without sinking.
[0047] Example 4:
[0048] Sodium bicarbonate powder and sodium chloride were ground in advance; 10g of phenolic resin was weighed and poured into a 100mL beaker, 1mL of anhydrous ethanol was added to adjust the viscosity of the phenolic resin, and after stirring evenly, 5g of sodium chloride powder before and after grinding and 1g of pre-ground sodium bicarbonate were added, and stirred at room temperature for 30min; 1g of surfactant Span-80 and 0.5g of NL curing agent were added to the mixed solution, and stirred at room temperature for 30min until the mixed solution was completely dissolved, and the precursor solution was prepared.
[0049] After the prepared solution has been allowed to stand until it is stable and no longer foams at room temperature, it is poured into a mold and then placed in a vacuum drying oven for foaming and curing. The temperature of the drying oven is set to 90℃ and left for at least 48 hours to allow it to foam and cure completely.
[0050] After complete curing, demold and soak in warm water to drain the sodium chloride template from the precursor foam. Then place in a drying oven to dry.
[0051] After the phenolic foam is dried, the sample is carbonized by heating it to 1000℃ at a rate of 5℃ / min under argon protection and holding it for 3 hours to obtain non-graphitized carbon foam.
[0052] Figure 5 The electron scanning images show that after adding fine salt with smaller particle size, the carbon foam produced has smaller pore size and more abundant pores, with the pore size mainly distributed between 200-300 μm.
[0053] Example 5:
[0054] In this embodiment, compared with non-graphitized carbon foam at 1000℃, graphitized carbon foam was obtained by placing it in a high-temperature furnace and heating it to 2100℃ at a heating rate of 20℃ / min, and holding it at that temperature for 2 hours. Figure 6 The electron scanning image of graphitized carbon foam shows that it has a similar microstructure and pore structure to that of non-graphitized carbon foam.
[0055] Counterexample 1:
[0056] Sodium bicarbonate powder (foaming agent) and hexamethylenetetramine (curing agent) were ground in advance. 10g of phenolic resin was weighed and poured into a 100mL beaker. 1mL of anhydrous ethanol was added to adjust the viscosity of the phenolic resin. After stirring evenly, 10g of sodium chloride powder and 0.1g of pre-ground sodium bicarbonate were added. The mixture was stirred at room temperature for 30min. 1g of surfactant Tween-80 and 0.5g of curing agent hexamethylenetetramine were added to the mixed solution. The mixture was stirred at room temperature for 30min until the mixed solution was completely dissolved. The precursor solution was then prepared.
[0057] After the prepared solution has been allowed to stand until it is stable and no longer foams at room temperature, it is poured into a mold and then placed in a drying oven for foaming and curing. The temperature of the drying oven is set to 150℃ and left for at least 48 hours to allow it to cure completely.
[0058] After complete curing, demold and soak in warm water to drain the sodium chloride template from the precursor foam. Then place in a drying oven to dry for 24 hours.
[0059] After the phenolic foam was dried, the sample was carbonized by heating it to 600℃ at a rate of 5℃ / min under argon protection and holding it at that temperature for 0.5h to obtain non-graphitized carbon foam. The prepared carbon foam had uneven pore distribution and porosity, and the pore shape was not completely globalized, with most of it retaining the shape of sodium chloride particles.
[0060] In summary, the method for preparing porous carbon by combining template method and foaming method provided by this invention can produce porous carbon materials with uniform pore structure and adjustable pore size. The carbon foam structure can be controlled by adjusting the content of foaming agent and template and the heat treatment regime. Compared with other methods, it is simple to operate, safe and non-toxic, low in cost and widely used, and suitable for large-scale industrial production.
Claims
1. A method for synthesizing porous carbon using a template method combined with a foaming method, characterized in that, Includes the following steps: A uniform mixed solution is obtained by mixing and stirring carbon-rich resin, water-soluble salt template, foaming agent, surfactant, and curing agent according to a set ratio; the water-soluble salt template is NaCl, the foaming agent is NaHCO3 powder, and the NaHCO3 powder needs to be ground before being added; the curing agent is powder particles, and the curing agent powder particles need to be ground before being added; the surfactant is Tween-80 or Span-80. The mixed solution is poured into a mold to foam and solidify. After demolding, the organic precursor foam is obtained. The NaCl template is removed before subsequent heating and carbonization to avoid cracking caused by the difference in thermal expansion coefficients between NaCl and resin foam during the carbonization process. The organic precursor foam was soaked in water to remove water-soluble salt templates and then dried to obtain a porous carbon precursor. Then, the material is heated and carbonized in an inert atmosphere to obtain a porous carbon foam material with a porosity of up to 80% and uniform distribution; the inert atmosphere is argon or nitrogen, the carbonization temperature is 650-1000℃, the heating rate is 5℃ / min, and the holding time is 0.5-3h.
2. The method for synthesizing porous carbon by combining template method with foaming method according to claim 1, characterized in that, The carbon-rich resin is a phenolic resin, epoxy resin, or silicone resin.
3. The method for synthesizing porous carbon by combining template method with foaming method according to claim 1, characterized in that, The mass ratio of the carbon-rich resin, water-soluble salt template, foaming agent, surfactant, and curing agent is 10-20:1-20:1-3:1-5:0.5-5.
4. The method for synthesizing porous carbon by combining template method with foaming method according to claim 1, characterized in that, Curing is carried out under heating conditions. The precursor solution is cured and foamed using a vacuum drying oven, forced-air drying oven, water bath, oil bath, or heating table. The curing temperature is 50-150℃, and the treatment time is at least 48 hours.
5. The method for synthesizing porous carbon by combining template method with foaming method according to claim 1, characterized in that, Porous graphite materials are obtained by directly graphitizing organic precursor foam during heat treatment, or by graphitizing it again after carbonization.
6. The method for synthesizing porous carbon by combining template method with foaming method according to claim 1, characterized in that, Porous carbon of a specified size or shape can be obtained by designing molds, cutting and polishing organic precursor foams, or cutting and polishing carbonized products.
Citation Information
Patent Citations
Preparation method of self-supporting three-dimensional porous carbon foam
CN115477548A
Preparation method of foam carbon with sodium bicarbonate as foaming agent
CN116081596A