Preparation method of a cement binder castable accelerator and application thereof

By preparing fine hydration products as accelerators for hydration crystal nuclei, the problems of high difficulty in controlling existing accelerators and high cost are solved, achieving efficient solidification and strength improvement of cement-bonded castables, which is suitable for the production of calcium aluminate cement-bonded castables.

CN118420260BActive Publication Date: 2026-11-20ZHENGZHOU UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410329052.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-21
Publication Date
2026-11-20
Estimated Expiration
2044-03-21

AI Technical Summary

Technical Problem

Existing accelerators are difficult to control in terms of dosage, easily leading to flash setting of castables, and have high production costs, are environmentally unfriendly, and have insignificant accelerating effects, especially at low temperatures.

Method used

A metal chloride salt solution is mixed with cement, and after filtration, freeze drying and ball milling, a grinding aid is added to prepare a setting accelerator, which generates fine hydration products as hydration nuclei to promote cement hydration.

Benefits of technology

It effectively shortens the setting time of cement-bonded castables, improves demolding and drying strength, is easy to control the amount added, reduces production costs, and is environmentally friendly and efficient.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004752921440000061
    Figure BDA0004752921440000061
  • Figure BDA0004752921440000062
    Figure BDA0004752921440000062
  • Figure BDA0004752921440000081
    Figure BDA0004752921440000081
Patent Text Reader

Abstract

The application belongs to the technical field of building materials, and particularly relates to a preparation method of a cement combined castable accelerator. The steps of the preparation method are as follows: (1) a metal chloride solution is added into cement, and stirring is performed to obtain mixed slurry; (2) the mixed slurry prepared in step (1) is filtered to obtain filter cake, and the filter cake is sequentially subjected to freezing and drying under vacuum to obtain powder; and (3) the powder prepared in step (2) is mixed with a grinding aid, and then grinding is performed to obtain the cement combined castable accelerator. The accelerator prepared by the application can not only shorten the setting time of calcium aluminate cement combined castable, but also improve the demolding strength and dry strength of the cement combined castable, greatly improving the production efficiency and economic benefits of the cement combined castable prefabricated part, and having great commercial application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of building materials technology, specifically to a method for preparing an accelerator for cement-bonded castables and its application. Background Technology

[0002] Calcium aluminate cement (CAC) is a commonly used binder in castables, possessing excellent physicochemical properties such as rapid setting and hardening, good corrosion resistance, and high wear resistance. Castable construction includes casting, curing, drying, and baking. Curing involves storing the castable at a specific temperature for a period of time, allowing the CAC binder inside to gradually hydrate, providing early strength. In actual production, the demolding strength of the castable ensures that the sample remains intact upon removal from the mold. Therefore, faster cement hydration, improving the demolding strength of the castable, can shorten the demolding time, improving production efficiency and economic benefits for the production of large CAC-bonded castable precast components. Therefore, in actual production, introducing accelerators to promote cement hydration and thus improve the demolding and drying strength of the castable is particularly important.

[0003] The hydration process of calcium aluminate cement is essentially a reaction between a low-solubility solid and water to form a solid product with even lower solubility, which can be divided into three stages: dissolution, nucleation, and precipitation. Among these, dissolution and nucleation are the key factors limiting cement hydration. Currently used accelerators primarily work by introducing certain ions to change the ion concentration in the castable solution, thereby promoting the dissolution of cement particles and the hydration of the castable, thus achieving an accelerated setting effect. For example, taking the introduction of some common lithium compounds as an example, after introducing lithium salts, the dissolved Li... + This will form insoluble hydroxides, such as LiAl(OH)4, causing Al(OH) in the solution to become insoluble. 4- The concentration decreases. Promoting further dissolution of cement particles causes a further change in the stoichiometry of dissolved ions in the solution, thus accelerating the dissolution process and promoting cement hydration. However, the amount of this accelerator added is difficult to control during construction. When its content is high, it may cause "flash setting" of the castable, which is detrimental to its construction. Furthermore, because the solubility of this accelerator is greatly affected by temperature, the accelerating effect at low concentrations is not significant at lower temperatures.

[0004] Chinese invention patent application CN113045298A discloses a method for preparing an alumina-based accelerator for refractory castables. Using industrial alumina as the main raw material, the method involves calcining at 900–1100℃ and cooling to room temperature to obtain alumina powder with a high specific surface area. Propylene glycol is then added as a grinding aid, and the mixture is dry-milled using a ball milling process to obtain alumina micro-powder with a high specific surface area. The essence of this accelerator is to provide small-particle "impurities" during the nucleation stage of cement hydration, resulting in "non-uniform nucleation" of the hydration products. However, due to the significant difference in crystal structure between the introduced alumina micro-powder and the hydration products, the "nucleation rate" of the nucleation process is not high, and the accelerating effect is not significant. Furthermore, the production process of this accelerator requires high-temperature calcination at 900–1100℃, which is costly and detrimental to environmental protection and resource conservation.

[0005] Therefore, there is an urgent need to study a low-cost accelerator that is easy to control in terms of its addition amount, easy to promote cement nucleation, and does not require calcination. Summary of the Invention

[0006] In view of the problems and shortcomings of the existing technology, the purpose of this invention is to provide a method for preparing an accelerator for cement-bonded castables and its application.

[0007] To achieve the objectives of this invention, the technical solution adopted is as follows:

[0008] The first aspect of this invention provides a method for preparing an accelerator for cement-bonded castables, comprising the following steps:

[0009] (1) Add the metal chloride salt solution to the cement and stir to mix well to obtain a mixed slurry;

[0010] (2) The mixed slurry prepared in step (1) is filtered to obtain a filter cake; the filter cake is then frozen and dried under vacuum to obtain a powder.

[0011] (3) The powder obtained in step (2) is mixed evenly with the grinding aid and then ground to obtain a accelerator for cement-bonded castable.

[0012] According to the above preparation method, preferably, the metal chloride salt in step (1) is at least one of potassium chloride, sodium chloride, and magnesium chloride. More preferably, the metal chloride salt is sodium chloride.

[0013] According to the above preparation method, preferably, the concentration of metal chloride in the metal chloride solution in step (1) is 0-180 g / L; more preferably, the concentration of metal chloride in the metal chloride solution is 10-150 g / L; most preferably, the concentration of metal chloride in the metal chloride solution is 30-150 g / L.

[0014] According to the preparation method described above, preferably, the mass ratio of the cement to the metal chloride solution is 1:2 to 10; more preferably, the mass ratio of the cement to the metal chloride solution is 1:5.

[0015] According to the above preparation method, preferably, the grinding aid in step (3) is any one of polymeric polyol, polymeric alkanolamine, triethanolamine, ethylene glycol, propylene glycol, and glycerol. More preferably, the grinding aid is a polymeric polyol. Most preferably, the grinding aid is polymeric polyol HE-a (purchased from Luoyang Hongen New Building Materials Co., Ltd., product model HE-a), which has good grinding aid effect and early strength increase effect.

[0016] According to the above preparation method, preferably, the amount of the grinding aid accounts for 0% to 0.2% of the total weight of the powder; more preferably, the amount of the grinding aid accounts for 0% to 0.15% of the total weight of the powder; most preferably, the amount of the grinding aid accounts for 0% to 0.1% of the total weight of the powder.

[0017] According to the above preparation method, preferably, the stirring temperature in step (1) is 0-60°C; more preferably, the stirring temperature is 5-60°C; and most preferably, the stirring temperature is 10-40°C.

[0018] According to the above preparation method, preferably, in step (1), the stirring time is 1 to 10 hours and the stirring rate is 500 to 2000 r / min; more preferably, the stirring time is 5 hours and the stirring rate is 1000 r / min.

[0019] According to the above preparation method, preferably, in step (2), the freezing temperature is -20℃ to -40℃ and the freezing time is 30 to 120 min; more preferably, the freezing temperature is -40℃ and the freezing time is 60 min.

[0020] According to the above preparation method, preferably, in step (2), the drying temperature is 40℃~100℃ and the drying time is 6~12h; more preferably, the drying temperature is 40℃ and the drying time is 6h.

[0021] According to the above preparation method, preferably, in step (2), the vacuum degree of the vacuum condition is 10 to 30 Pa; more preferably, the vacuum degree is 20 Pa.

[0022] According to the above preparation method, preferably, the grinding method in step (3) is ball milling, the ball-to-material ratio is 1 to 4:1, the ball milling time is 0.5 to 4 hours, and the rotation speed of the ball mill is 50 to 400 r / min.

[0023] According to the above preparation method, preferably, the cement is aluminate cement; more preferably, the cement is calcium aluminate cement; even more preferably, the alumina content in the cement is 50% to 80%; most preferably, the cement is at least one of CA50, CA-60, CA-70, and CA-80 (as specified in national standard GB / T201-2015).

[0024] According to the above preparation method, preferably, the filtration in step (2) is vacuum filtration; more preferably, the vacuum filtration pressure is less than 0.07 MPa, the filter membrane pore size used during filtration is 5 to 20 μm, and the filtration time is 5 to 30 min.

[0025] According to the above preparation method, preferably, the D50 particle size of the accelerator for cement-bonded castable is 10-20 μm.

[0026] A second aspect of the present invention provides a coagulant product prepared using the preparation method described in the first aspect above.

[0027] The third aspect of the present invention provides the application of the accelerator product described in the second aspect above in cement-bound castables.

[0028] A fourth aspect of the present invention provides a cement-bonded castable containing the accelerator product described in the second aspect above.

[0029] The setting accelerator mechanism of the cement-bonded castable accelerator prepared in this invention is as follows:

[0030] Stirring calcium aluminate cement in a sodium chloride solution at a certain temperature for a period of time beforehand can cause the formation of fine hydration products (CAH) on the surface of the cement particles. 10 The fine hydration products, either C2AH8 or C3AH6, are filtered and freeze-dried under vacuum to preserve them. After grinding with the addition of a grinding aid, the fine hydration products on the particle surface are removed, resulting in a setting accelerator containing fine hydration products. When the prepared setting accelerator is introduced into the castable, the introduced fine hydration products can serve as nuclei during the hydration process of cement in the castable. Moreover, since the introduced nuclei have the same structure as the hydration products, they can promote the rapid nucleation of hydration products, which then precipitate to form hydration products, providing strength to the castable and promoting its setting.

[0031] Compared with the prior art, the positive and beneficial effects achieved by the present invention are as follows:

[0032] (1) The accelerator of the present invention can effectively promote the solidification of calcium aluminate cement-bonded castables. Compared with cement-bonded castables without accelerator, the initial setting time of cement-bonded castables with the addition of the accelerator of the present invention is shortened from about 5 hours to 2-3 hours, and the final setting time is shortened from about 17 hours to 4-5 hours. At the same time, the accelerator of the present invention can effectively improve the demolding strength and drying strength of cement-bonded castables. Compared with cement-bonded castables without accelerator, the flexural strength and compressive strength of cement-bonded castables after demolding after 24 hours of curing with the accelerator of the present invention are increased by about 55% and 81%, respectively. Moreover, the flexural strength and compressive strength of cement-bonded castables after curing and drying are increased by about 48% and 31%, respectively. Therefore, the accelerator prepared by the present invention can not only shorten the setting time of calcium aluminate cement-bonded castables, but also improve the demolding strength and drying strength of cement-bonded castables, which greatly improves the production efficiency and economic benefits of cement-bonded castable precast components and has great commercial application value.

[0033] (2) The amount of the accelerator added during the use of the present invention is easy to control. It can effectively promote cement hydration when the amount of low content is added, and will not cause the castable to "flash set" when the amount of high content is added, thus affecting the construction of the castable.

[0034] (3) The raw materials of the coagulant prepared by the present invention are easy to obtain, low in cost, simple to prepare, convenient to construct, and do not require high temperature calcination and other process conditions, thus saving resources, protecting the environment, and facilitating large-scale promotion and use. Attached Figure Description

[0035] Figure 1 The graph shows the particle size distribution results of the coagulants prepared in Examples 1-4.

[0036] Figure 2 SEM images of the coagulants prepared in Examples 1-4, 2-1, and 2-2 before ball milling; where a is Example 2-1, b is Example 1-4, and c is Example 2-2;

[0037] Figure 3 The hydration heat curves are for P0 and P1 during the curing process. Detailed Implementation

[0038] To enable those skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below with reference to specific embodiments.

[0039] The following detailed description is exemplary and intended to provide further illustration of the invention. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains.

[0040] It should be noted that the terminology used herein is for the purpose of describing specific embodiments only and is not intended to limit the exemplary embodiments of the present invention. Experimental methods in the following embodiments, unless otherwise specified, employ conventional techniques in this art or follow the conditions recommended by the manufacturer; reagents or instruments whose manufacturers are not specified are all commercially available conventional products.

[0041] Example 1: Investigation of the concentration of metal chloride salt solution

[0042] To investigate the effect of chloride solution concentration on the performance of the coagulant in the preparation method of the coagulant, experiments were conducted in Examples 1-1 to 1-5. The specific details of Examples 1-1 to 1-5 are as follows:

[0043] Example 1-1:

[0044] A method for preparing a setting accelerator for cement-bonded castables, comprising the following steps:

[0045] (1) Add sodium chloride solution to calcium aluminate cement and stir and mix evenly using a magnetic stirrer at 25°C to obtain a mixed slurry; wherein, the concentration of sodium chloride solution is 0 g / L, the mass ratio of calcium aluminate cement to sodium chloride solution is 1:5, the stirring time is 5 h, the stirring speed is 1000 r / min, and the calcium aluminate cement is Secar71 calcium aluminate cement.

[0046] (2) The mixed slurry prepared in step (1) is vacuum filtered to obtain a filter cake. The filter cake is then frozen and dried sequentially under a vacuum of 20 Pa to obtain a powder. The vacuum filtration pressure is 0.04 MPa, and the filter paper used for vacuum filtration has a pore size of 20 μm. The freezing temperature is -40℃ and the freezing time is 60 min. The drying temperature is 40℃ and the drying time is 6 h.

[0047] (3) The powder obtained in step (2) is mixed evenly with the grinding aid, and then ball milled using a ball mill to obtain the accelerator for cement-bonded castables; wherein the grinding aid is a polymeric polyol HE-a (purchased from Luoyang Hongen New Building Materials Co., Ltd., product model HE-a), the amount of polymeric polyol added accounts for 0.05% of the total weight of the powder, the ball-to-powder ratio during the ball milling process is 1 to 4:1, the ball milling time is 2 hours, and the rotation speed of the ball mill is 50 to 400 r / min.

[0048] The contents of Examples 1-2 to 1-5 are basically the same as those of Example 1-1, except that the concentration of sodium chloride solution in step (1) is different; the concentrations of sodium chloride in step (1) of Examples 1-2 to 1-5 are 30 g / L, 50 g / L, 100 g / L and 150 g / L, respectively.

[0049] The particle size analysis results of the accelerators for cement-bonded castables prepared in Examples 1-4 are as follows: Figure 1 As shown.

[0050] Depend on Figure 1 It can be seen that the particle size distribution of the prepared accelerator is unimodal, with the D10 particle size being 1.977 μm, the D50 particle size being 13.51 μm, and the D90 particle size being 38.40 μm. This indicates that after grinding, the particle size of the accelerator has reached the target level and can be used in cement-bound castables.

[0051] To test the setting-accelerating effect of the accelerators prepared in Examples 1-1 to 1-5 on cement-bonded castables, the accelerators prepared in Examples 1-1 to 1-5 were added to cement-bonded castables respectively, resulting in five types of cement castables, named castables S1, S2, S3, S4, and S5. A cement castable without added accelerators was also prepared and named S0. The six types of castables prepared above were poured into 40mm×40mm×160mm molds and placed on a GZ-85 vibrating table for vibration molding. The samples were then placed in a constant temperature and humidity curing chamber at 25℃ for 24 hours. The initial setting time and final setting time were measured according to standard GB / T1346-2011.

[0052] The raw materials for cement-bonded castables are: aggregates (tabular corundum with different particle size distributions, 0-0.5mm, 0.5-1mm, 1-3mm, 3-6mm, Al2O3≥99%, Shandong Hengjia Co., Ltd.), tabular corundum fine powder (≤0.045mm, Shandong Hengjia Co., Ltd.), α-Al2O3 micro powder (CL370, Anmai Aluminum (Qingdao) Co., Ltd.), calcium aluminate cement Secar71 (Tianjin Kainuos), and water-reducing agents (ADW1 and ADS3, Anmai Aluminum (Qingdao) Co., Ltd.). The formulation of the cement-bonded castable is shown in Table 1.

[0053] The preparation method of cement-bonded castable is as follows: weigh each raw material according to the raw material composition in the castable formula, add the raw materials except water to the mortar mixer and dry mix for 60 seconds, then add water and mix for 180 seconds to obtain cement-bonded castable.

[0054] Table 1 Formulations of castable samples S0-S5

[0055]

[0056] The initial setting time and final setting time test results of castable samples S0, S1, S2, S3, S4 and S5 are shown in Table 2.

[0057] Table 2 Test results of castable samples S0 to S5

[0058]

[0059] As shown in Table 2, compared with cement-bonded castables without accelerators, the initial setting time and final setting time of the castables were significantly shortened after adding 1% of the accelerators prepared in Examples 1-1 to 1-5 of this invention to the cement-bonded castables. Furthermore, as the concentration of sodium chloride solution in the accelerator increased, the initial setting time and final setting time of the castables gradually shortened. When the concentration of sodium chloride in the accelerator was 100 g / L, the initial setting time and final setting time reached their shortest values ​​of 2.3 h and 4.8 h, respectively. The reason is that during the preparation process, when a strong electrolyte (sodium chloride) that does not share the same ions as the weak electrolyte is added to the solution of the weak electrolyte, the total ion concentration in the solution increases, and the mutual restraint between ions is enhanced. This reduces the chance of the anions and cations from the dissociation of the weak electrolyte combining to form molecules, thus decreasing the concentration of weak electrolyte molecules and correspondingly increasing the ion concentration and degree of dissociation. Therefore, the dissolution of sodium chloride increases the total ion concentration in the solution, reducing the chance of ions generated from cement dissolution combining to form molecules, allowing the cement to dissolve further, promoting cement hydration in the solution, and generating more hydration products on the surface of cement particles. This results in a better setting accelerator. The above results show that the setting accelerator prepared by this invention can effectively promote the solidification of cement-bonded castables, shorten the solidification time of cement castables, and greatly improve the production efficiency of cement-bonded castable precast components. Moreover, the concentration of sodium chloride solution in the setting accelerator is preferably 30-150 g / L, more preferably 50-150 g / L, and most preferably 100 g / L.

[0060] Example 2: Experiment exploring the stirring temperature

[0061] To investigate the effect of stirring temperature on the performance of the coagulant during its preparation, experiments were conducted in Examples 2-1 to 2-2. The specific details of Examples 2-1 to 2-2 are as follows:

[0062] Example 2-1:

[0063] A method for preparing a setting accelerator for cement-bonded castables, comprising the following steps:

[0064] (1) Add 100 g / L sodium chloride solution to calcium aluminate cement, the mass ratio of calcium aluminate cement to sodium chloride solution is 1:5, and stir evenly with a magnetic stirrer to obtain a mixed slurry; wherein, the stirring temperature is 10℃, the stirring time is 5 h, the stirring speed is 1000 r / min, and the calcium aluminate cement is calcium aluminate cement Secar71.

[0065] (2) The mixed slurry prepared in step (1) is vacuum filtered to obtain a filter cake. The filter cake is then frozen and dried sequentially under a vacuum of 20 Pa to obtain a powder. The vacuum filtration pressure is 0.04 MPa, and the filter paper used for vacuum filtration has a pore size of 20 μm. The freezing temperature is -40℃ and the freezing time is 60 min. The drying temperature is 40℃ and the drying time is 6 h.

[0066] (3) The powder obtained in step (2) is mixed evenly with the grinding aid, and then ball milled using a ball mill to obtain the accelerator for cement-bonded castables; wherein the grinding aid is a polymeric polyol HE-a (purchased from Luoyang Hongen New Building Materials Co., Ltd., product model HE-a), the amount of polymeric polyol added accounts for 0.05% of the total weight of the powder, the ball-to-powder ratio during the ball milling process is 1 to 4:1, the ball milling time is 2 hours, and the rotation speed of the ball mill is 50 to 400 r / min.

[0067] The contents of Examples 2-2 to 2-5 are basically the same as those of Example 2-1, except that the stirring temperature in step (1) is 40℃, 60℃, 0℃, and -5℃.

[0068] To test the setting-accelerating effect of the accelerators prepared in Examples 2-1 to 2-5 on cement-bonded castables, the accelerators prepared in Examples 2-1 to 2-5 were added to cement-bonded castables respectively, resulting in two types of cement castables, named castables S6, S7, S8, S9, and S10. The two types of castables prepared above were poured into 40mm×40mm×160mm molds and placed on a GZ-85 vibrating table for vibration molding. The samples were then placed in a constant temperature and humidity curing chamber at 25℃ for 24 hours, and their initial setting time and final setting time were measured according to standard GB / T1346-2011.

[0069] The raw materials of the cement-bonded castable are the same as those in Example 1. The formula of the cement-bonded castable is shown in Table 3. The preparation method of the cement-bonded castable is the same as that in Example 1.

[0070] Table 3 Formulations of castable samples S6 to S10

[0071]

[0072] The initial setting time and final setting time test results of castable samples S0, S6, S7, S8, S9 and S10 are shown in Table 4.

[0073] Table 4 Test results of castable samples S6 to S10

[0074]

[0075]

[0076] As shown in Table 4, compared with cement-bonded castables without accelerators, the initial and final setting times of the castables were significantly shortened after adding 1% of the accelerators prepared in Examples 2-1 to 2-3 of this invention. Furthermore, with increasing stirring temperature, both the initial and final setting times of the castables first decreased and then increased, reaching their shortest values ​​of 2.3 h and 4.8 h at a stirring temperature of 25°C. This is because calcium aluminate cement hydrates after being added to sodium chloride solution, and the hydration products differ at different stirring temperatures. At a stirring temperature of 60°C, the accelerator's setting effect was not significantly different from that of the accelerator prepared in Example 2-2 (stirring temperature 40°C). This may be because the hydration products did not change after the stirring temperature exceeded 40°C, and the hydration products generated at 40°C had already reached their maximum value.

[0077] Furthermore, compared with cement-bonded castables without accelerators, the initial setting time and final setting time of the castables did not change significantly after adding 1% of the accelerators prepared in Examples 2-4 to 2-5 of this invention to the cement-bonded castables. This is because the stirring temperature was low when the accelerators were prepared in Examples 2-4 and 2-5. At this time, when the sodium chloride and calcium aluminate cement mixture was stirred, the calcium aluminate cement in the mixture did not undergo hydration due to the low temperature, so no hydration products were generated, and the prepared accelerators had no effect.

[0078] SEM images of the dried powder of the coagulants prepared in Examples 2-1, 2-2, and 1-4 before ball milling are shown below. Figure 1 As shown. By Figure 1 It can be seen that the hydration product generated in Example 2-1 at a stirring temperature of 10°C is mainly needle-shaped CAH. 10In Examples 2-2, the hydration products generated at a stirring temperature of 40°C were mainly granular C3AH6, while in Examples 1-4, the hydration products generated at a stirring temperature of 25°C were mainly plate-like C2AH8. These hydration products remained in the accelerator after ball milling. When the accelerator was introduced into the castable, the fine hydration product particles provided nuclei for the hydration of cement in the castable, which was beneficial to further hydration of cement and achieved the accelerating effect. Moreover, since the plate-like hydration product C2AH8 generated at a stirring temperature of 25°C could serve as the nuclei for cement hydration during the curing process of the castable, its accelerating effect was the best.

[0079] Example 3: Discussion on the Dosage of Polymerized Polyols

[0080] To investigate the effect of the amount of technically polymerized polyol used in the preparation method of the coagulant on the performance of the coagulant, experiments were conducted in Examples 3-1 and 3-2. The specific details of Examples 3-1 and 3-2 are as follows:

[0081] Example 3-1:

[0082] A method for preparing a setting accelerator for cement-bonded castables, comprising the following steps:

[0083] (1) Add 100 g / L sodium chloride solution to calcium aluminate cement, the mass ratio of calcium aluminate cement to sodium chloride solution is 1:5, and stir evenly with a magnetic stirrer to obtain a mixed slurry; wherein, the stirring temperature is 25℃, the stirring time is 5 h, the stirring speed is 1000 r / min, and the calcium aluminate cement is calcium aluminate cement Secar71.

[0084] (2) The mixed slurry prepared in step (1) is vacuum filtered to obtain a filter cake. The filter cake is then frozen and dried sequentially under a vacuum of 20 Pa to obtain a powder. The vacuum filtration pressure is 0.04 MPa, and the filter paper used for vacuum filtration has a pore size of 20 μm. The freezing temperature is -40℃ and the freezing time is 60 min. The drying temperature is 40℃ and the drying time is 6 h.

[0085] (3) The powder obtained in step (2) is mixed evenly with the grinding aid, and then ball milled using a ball mill to obtain the accelerator for cement-bonded castables; wherein the grinding aid is a polymeric polyol HE-a (purchased from Luoyang Hongen New Building Materials Co., Ltd., product model HE-a), the amount of polymeric polyol added accounts for 0% of the total weight of the powder, the ball-to-powder ratio during the ball milling process is 1 to 4:1, the ball milling time is 2 hours, and the rotation speed of the ball mill is 50 to 400 r / min.

[0086] The content of Example 3-2 is basically the same as that of Example 3-1, except that the amount of polymerized polyol added in step (3) accounts for 0.1% of the total weight of the powder.

[0087] To test the setting-accelerating effect of the accelerators prepared in Examples 3-1 and 3-2 on cement-bonded castables, the accelerators prepared in Examples 3-1 and 3-2 were added to cement-bonded castables respectively, resulting in two types of cement castables, named castables S11 and S12. The two types of castables were poured into 40mm×40mm×160mm molds and vibrated on a GZ-85 type vibrating table. The samples were then placed in a constant temperature and humidity curing chamber at 25℃ for 24 hours. The initial setting time and final setting time were measured according to standard GB / T1346-2011.

[0088] The raw materials of the cement-bonded castable are the same as those in Example 1. The formula of the cement-bonded castable is shown in Table 5. The preparation method of the cement-bonded castable is the same as that in Example 1.

[0089] Table 5 Formulations of castable samples S11-S12

[0090]

[0091] The initial setting time and final setting time test results of castable samples S0, S11 and S12 are shown in Table 6.

[0092] Table 6 Test results of castable samples S11 to S12

[0093]

[0094] As shown in Table 6, compared with cement-bonded castables without accelerators, the initial and final setting times of the castables were significantly shortened after adding 1% of the accelerators prepared in Examples 3-1 to 3-2 of this invention. Furthermore, with the increase of the amount of polymeric polyol, both the initial and final setting times of the castables decreased and then stabilized. The accelerator effect was most significant when the amount of polymeric polyol added accounted for 0.05% of the total weight of the powder, with the shortest initial and final setting times of 2.3 h and 4.8 h, respectively. Further increasing the amount of polymeric polyol did not significantly change the initial and final setting times. This is because the use of polymeric polyol allows for better grinding of the hydration products on the surface of cement particles during ball milling, thus better exerting the accelerator effect in the castable. However, when the amount of polymeric polyol added was increased to 0.1%, the accelerator effect of the prepared accelerator was not significantly improved compared to adding 0.05% polymeric polyol. This indicates that the optimal amount of polymeric polyol added is 0.05% of the powder.

[0095] 1. The effect of the accelerator of this invention on the strength of calcium aluminate cement-bonded castables

[0096] Taking the cement-bonded castable sample S4 prepared in Example 1 as an example, the effect of the accelerator of the present invention on the strength of the castable was studied, while the cement-bonded castable sample S0 was used as a blank control.

[0097] Cement-bonded castable samples S4 and S0 were poured into a 40mm×40mm×160mm mold and placed on a GZ-85 vibrating table for vibration molding. The samples were then placed in a constant temperature and humidity curing chamber at 25℃ for 24 hours. The initial setting time and final setting time were measured according to standard GB / T1346-2011. After curing, the castable was demolded and placed in an oven (110℃) for drying for 24 hours. The room temperature flexural strength and room temperature compressive strength of the samples after curing and drying were then tested. The test results are shown in Table 7.

[0098] Table 7 Performance test results of castable samples S4 and S0

[0099] Sample number S0 S4 Initial setting time / h 4.7 2.3 Final setting time / h 17.0 4.8 Flexural strength after demolding after 24 hours of curing / MPa 5.9 9.1 Compressive strength after demolding after 24 hours of curing / MPa 40.1 72.3 Flexural strength after drying / MPa 18.2 26.9 Pressure resistance after drying / MPa 130 170.4

[0100] As shown in Table 7, after the accelerators prepared in Examples 1-4 were introduced into the castables, the demolding strength and drying strength of the castables increased significantly. This indicates that the accelerators not only have the effect of accelerating setting, but also help to promote the further hydration of calcium aluminate cement during the curing process, thereby improving the strength of the castables.

[0101] 2. The effect of the accelerator of this invention on the hydration of calcium aluminate cement

[0102] Taking the accelerators prepared in Examples 1-4 as examples, they were added to calcium aluminate cement paste. The amount of accelerators used in Examples 1-4 accounted for 20% of the total weight of calcium aluminate cement in the calcium aluminate cement paste. The effect of the prepared accelerators on the hydration rate of calcium aluminate cement was studied by measuring the hydration heat curves during the curing process of the calcium aluminate cement paste. At the same time, a blank control without accelerators was set up. The cement paste with accelerators prepared in Examples 1-4 was designated as P1, and the cement paste without accelerators was designated as P0. The cement paste was prepared by adding 50g of calcium aluminate cement (Secar-71 cement, Tianjin Kainuos) to 100g of deionized water and stirring until homogeneous.

[0103] The specific experimental steps for measuring the hydration heat curve of calcium aluminate cement paste during curing are as follows:

[0104] Prepare the cement paste in a plastic cup, then place the cup in an insulated container within a constant-temperature curing chamber. Cover the container and insert a thermocouple into the paste. The real-time temperature recording system (PTS-12S) of the hydration heat tester, connected to the thermocouple, records the real-time temperature change of the paste over time, thus obtaining the hydration heat release curve of the CAC paste at a curing temperature of 25℃. This reflects the cement hydration rate. The hydration heat curves of calcium aluminate cement paste during the P0 and P1 curing processes are shown below. Figure 2 As shown.

[0105] Depend on Figure 2 It is known that in calcium aluminate cement paste without the introduction of an accelerator, cement hydration only begins after 15 hours of curing, reaches its peak hydration heat release temperature after 18 hours of curing, and is completely hydrated after 20 hours of curing. However, with the addition of the accelerator prepared in Examples 1-4, calcium aluminate cement paste begins hydration after 2 hours of curing, reaches its peak hydration heat release temperature after 3.5 hours of curing, and is completely hydrated after 6 hours of curing. This indicates that the accelerator prepared in Examples 1-4 is beneficial for promoting the hydration of calcium aluminate cement.

[0106] Finally, it should be noted that the above embodiments are merely preferred embodiments of the present invention and are not intended to limit the present invention in any other way. Any person skilled in the art may use the above technical content as inspiration to make changes or modifications. These are equivalent embodiments with variations. However, any simple modifications, equivalent changes, and modifications made to the above embodiments based on the technical essence of the present invention without departing from the technical concept of the present invention still fall within the protection scope of the claims of the present invention.

Claims

1. A method for preparing an accelerator for cement-bonded castables, characterized in that, Includes the following steps: (1) Add the metal chloride solution to the cement and stir to mix evenly to obtain a mixed slurry; the metal chloride is at least one of potassium chloride, sodium chloride, and magnesium chloride; the concentration of the metal chloride in the metal chloride solution is 30-150 g / L; the mass ratio of the cement to the metal chloride solution is 1:2-10; the cement is aluminate cement; the stirring temperature is 10-40℃ and the stirring time is 1-10 h; (2) The mixed slurry prepared in step (1) is filtered to obtain a filter cake; the filter cake is frozen and dried under vacuum conditions to obtain powder; the freezing temperature is -20℃ to -40℃ and the freezing time is 30 to 120 min; the drying temperature is 40℃ and the drying time is 6 to 12 h. (3) After the powder obtained in step (2) is mixed evenly with the grinding aid, it is ground to obtain the accelerator for cement-bonded castable.

2. The preparation method according to claim 1, characterized in that, The grinding aid mentioned in step (3) is any one of polymeric polyol, polymeric alcohol amine, triethanolamine, ethylene glycol, propylene glycol, and glycerol.

3. The preparation method according to claim 2, characterized in that, The grinding aid is used in an amount of 0% to 0.2% of the total weight of the powder.

4. A coagulant product prepared by any one of the preparation methods described in claims 1 to 3.

5. The application of the accelerator product according to claim 4 in cement-bonded castables.

Citation Information

Patent Citations

  • Alumina-based coagulant for refractory castable as well as preparation method and application of alumina-based coagulant

    CN113045298A

  • Method for prepn. of cement coagulant and application thereof

    CN1120525A