A high-temperature-resistant copper alloy with high strength and toughness and a preparation method thereof

By introducing Cr, Ti, Zr, and Zn elements into Cu-Ni-Al alloys and employing grain boundary strengthening and precipitation strengthening methods, high-temperature stable Cu-Ni-Al-Cr-Ti-Zr-Zn alloys were prepared, solving the problems of insufficient elongation and electrical conductivity of the alloys at high temperatures and achieving a significant improvement in high-temperature performance.

CN118422006BActive Publication Date: 2026-11-24DALIAN UNIV OF TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410604284.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-15
Publication Date
2026-11-24
Estimated Expiration
2044-05-15

AI Technical Summary

Technical Problem

Existing Cu-Ni-Al alloys exhibit discontinuous precipitation at grain boundaries under high-temperature conditions, resulting in poor alloy elongation, decreased electrical conductivity, and insufficient microstructural stability, thus limiting their application in high-temperature scenarios.

Method used

By introducing Cr, Ti, Zr, and Zn elements to promote γ' phase strengthening, and employing grain boundary strengthening and precipitation strengthening, Cu-Ni-Al-Cr-Ti-Zr-Zn alloys were prepared. The elemental composition and heat treatment process were optimized to improve the high-temperature microstructure stability and overall performance of the alloys.

Benefits of technology

At 600℃, the alloy exhibits high strength (not less than 371MPa), high elongation (not less than 3.7%) and high electrical conductivity (not less than 18.4% IACS), which are significantly better than those of commercially available copper alloys. Moreover, the preparation method is highly repeatable and low in cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118422006B_ABST
    Figure CN118422006B_ABST
Patent Text Reader

Abstract

A high-strength and high-toughness Cu-Ni-Al-Cr-Ti-Zr-Zn high-temperature resistant copper alloy with stable structure belongs to the field of high-temperature copper alloys. The alloy's mass percentage composition is: Cu: 83.67~87.67wt%, Ni: 8.55~12.55wt%, Al: 0.81~1.51wt%, Cr: 0.67~1.07wt%, Ti: 0.61~1.01wt%, Zr: 0.32~0.72wt%, Zn: 0.27~0.47wt%. In its aged state, the alloy exhibits a room temperature hardness of 297±17.8 Hv, a tensile strength of not less than 819 MPa, an elongation of not less than 11.1%, and an electrical conductivity of not less than 18.4% IACS; at 600℃, the hardness is 192±13.5 Hv, the tensile strength is not less than 371 MPa, and the elongation is not less than 3.7%. After being held at 600℃ for 400 hours, the hardness of the alloy varied within 292±8.8Hv. Compared with commercial alloys, it exhibited good high-temperature performance and structural stability, and the conventional preparation method ensured high repeatability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a high-strength and high-toughness Cu-Ni-Al-Cr-Ti-Zr-Zn high-temperature resistant copper alloy with stable structure and its preparation method, which belongs to the field of high-temperature resistant copper alloys. Background Technology

[0002] Precipitation-strengthened copper alloys possess excellent strength, elongation, and electrical conductivity, making them widely used in electronics, communications, rail transportation, and aerospace. With the rapid development of these industries, higher demands are being placed on the temperature resistance of copper alloys. However, traditional precipitation-strengthened copper alloys are generally used below 600℃. Above 600℃, microstructural transformations such as the dissolution or growth of strengthening phases, grain growth, and the formation of harmful phases occur, leading to a sharp decline in performance and limiting their application in high-temperature environments. Currently, introducing cubic coherent γ'-Ni3Al phases has been proven to be an effective means of improving the high-temperature resistance of copper alloys. However, existing high-temperature resistant Cu-Ni-Al series alloys face challenges such as discontinuous precipitation (coarsening) at grain boundaries under high-temperature conditions and poor elongation due to high-density coherent precipitate interfaces. Furthermore, due to the miscibility of Cu and Ni, the large amount of Ni dissolved in Cu leads to a decrease in alloy electrical conductivity; simultaneously, the large amount of Cu dissolved in the γ' phase results in a certain degree of decrease in microstructural stability at high temperatures. Therefore, in order to expand the application of alloys in a wide temperature range, how to improve the elongation and electrical conductivity of alloys while maintaining their high-temperature performance and improving their high-temperature microstructure stability has become an urgent problem to be solved. Summary of the Invention

[0003] To address the problems existing in current Cu-Ni-Al alloys, this invention aims to prepare a precipitation-strengthened multi-component Cu-Ni-Al-Cr-Ti-Zr-Zn alloy with good high-temperature microstructure stability and comprehensive performance at both normal and high temperatures.

[0004] By utilizing the differences in mixing enthalpy between elements, solid solution of γ' phase strengthening elements is promoted in the γ' phase, thereby improving the high-temperature stability of the γ' phase. Introducing grain boundary strengthening elements enhances the alloy's strength and elongation, while simultaneously promoting the precipitation of alloying elements to improve electrical conductivity. By employing multiple mechanisms, including grain boundary strengthening and precipitation strengthening, the overall performance of the alloy at both room temperature and high temperatures is comprehensively improved.

[0005] To achieve the above objectives, the technical solution of the present invention is as follows: a high-strength and high-toughness Cu-Ni-Al-Cr-Ti-Zr-Zn high-temperature resistant copper alloy with stable structure has the following mass percentage composition: Cu: 83.67-87.67 wt%, Ni: 8.55-12.55 wt%, Al: 0.81-1.51 wt%, Cr: 0.67-1.07 wt%, Ti: 0.61-1.01 wt%, Zr: 0.32-0.72 wt%, Zn: 0.27-0.47 wt%, with the balance being unavoidable impurities.

[0006] The preparation method of a high-strength and high-toughness Cu-Ni-Al-Cr-Ti-Zr-Zn high-temperature resistant copper alloy with stable structure:

[0007] Based on the above composition of the alloy, the alloy is prepared using high-purity metals of 4N or higher as raw materials; a non-consumable vacuum arc melting furnace is used, and high-purity argon gas is introduced for protection, and the raw materials prepared according to the above alloy composition are repeatedly melted to finally obtain an alloy ingot with uniform composition; then the melted alloy ingot is subjected to solution treatment (cold rolling) and aging treatment to obtain a high-strength and high-toughness Cu-Ni-Al-Cr-Ti-Zr-Zn high-temperature resistant copper alloy with stable structure.

[0008] Preferably, the alloy ingot is subjected to solution treatment and aging treatment, followed by hardness and electrical conductivity testing; after the alloy ingot is cold rolled to eliminate casting defects, it is subjected to tensile strength testing after the same solution treatment and aging treatment.

[0009] Preferably, the solution treatment temperature in the above steps is 1020℃~1070℃, the time is 3~6h, and then the solution is quenched to room temperature.

[0010] Preferably, the aging treatment temperature in the above steps is 600-700℃, the time is 3-6 hours, and then the water is quenched to room temperature.

[0011] Preferably, the cold rolling process described in the above steps involves reducing the pressure by no more than 20% per pass, with multiple passes until the total pressure reaches 40% to 60%.

[0012] The alloy was subjected to room temperature and high temperature tensile tests using a universal testing machine; room temperature and high temperature hardness tests using a Vickers microhardness tester; and electrical conductivity tests using an eddy current conductivity meter.

[0013] The copper alloy obtained by the above preparation method has an aged room temperature hardness of 297±17.8 Hv, a tensile strength of not less than 819 MPa, an elongation of not less than 11.1%, and an electrical conductivity of not less than 18.4% IACS; at 600℃, the hardness is 192±13.5 Hv, the tensile strength is not less than 371 MPa, and the elongation is not less than 3.7%. After a long-term holding at 600℃ for 400 hours, the hardness of the alloy varies within 292±8.8 Hv.

[0014] The beneficial effects of this invention are as follows: Cr and Zr are typical strengthening elements in high-strength, high-conductivity copper alloys. The abundant precipitation of Cr and Zr ensures good conductivity and strength of the alloy. Simultaneously, Zr is a commonly used grain boundary strengthening element in high-temperature alloys; its segregation at grain boundaries strengthens them. Ti promotes the precipitation of the γ' phase in Cu-based and Ni-based alloys with a γ+γ′ structure, increasing the dissolution temperature and high-temperature stability of the γ′ phase. Furthermore, Ti also inhibits discontinuous precipitation at grain boundaries. Zn has a solid solution strengthening effect in copper alloys; compared to other elements, Zn has a relatively small impact on the electrical conductivity of copper alloys. Zn promotes the precipitation of other elements in copper alloys, effectively improving both strength and electrical conductivity. Therefore, by considering the interaction between alloying elements in copper alloys and partially replacing alloying elements at Al and Ni positions, the discontinuous precipitation of the alloy is significantly suppressed under the interaction of multiple elements. At the same time, the addition of Ti promotes the precipitation of γ' phase and refines the size of γ' phase, thereby increasing the dissolution temperature of γ' phase. In addition, the segregation of Zr element at grain boundaries can increase grain boundary strength while hindering the diffusion of oxygen element along the grain boundaries. The addition of Cr element significantly enhances the alloy's resistance to high-temperature oxidation. Under the synergistic effect of these elements, the high-temperature performance of the alloy is effectively improved. Typically, commercially available copper alloys such as C15000, C16200, C71630, C54400, and C26000 have a tensile strength of only around 100 MPa at 600°C. C18100, with better temperature resistance, can achieve a tensile strength of around 250 MPa at 600°C. However, the alloy provided by this invention exhibits a strength of no less than 371 MPa at 600°C while maintaining an elongation of no less than 3.7%, demonstrating high-temperature performance far superior to currently used commercially available copper alloys. Furthermore, this invention employs a conventional preparation method, ensuring high repeatability and contributing to cost reduction and efficient production. Attached Figure Description

[0015] Figure 1 It is the Cu after aging treatment in Example 1 85.67 Ni 10.55 Al 1.21 Cr 0.87 Ti 0.81 Zr 0.52 Zn 0.37 (wt.%) Hardness change of alloy after holding at 600℃ for 400h.

[0016] Figure 2 It is the Cu after aging treatment in Example 1 85.67 Ni 10.55 Al 1.21 Cr 0.87 Ti 0.81 Zr 0.52 Zn 0.37 Hardness diagrams of (wt.%) alloys at room temperature, 200℃, 400℃, 500℃, and 600℃.

[0017] Figure 3 It is the Cu after aging treatment in Example 1 85.67 Ni 10.55 Al 1.21 Cr 0.87 Ti 0.81 Zr 0.52 Zn 0.37 Engineering stress-strain curves of (wt.%) alloys at room temperature and 600°C. Detailed Implementation

[0018] The technical solution proposed by the present invention will be further described in detail below with reference to the accompanying drawings and embodiments. Obviously, this embodiment is only a part of all embodiments, and the protection scope of the present invention is not limited to the described part.

[0019] Example 1 Cu 85.67 Ni 10.55 Al 1.21 Cr 0.87 Ti 0.81 Zr 0.52 Zn 0.37 Preparation of (wt.%) alloys

[0020] Alloy preparation includes the following steps:

[0021] 1. Based on the alloy composition Cu 85.67 Ni 10.55 Al 1.21 Cr 0.87 Ti 0.81 Zr 0.52 Zn 0.37 (wt.%), using Cu and Al with a purity of 99.999wt.% and Ni, Ti, Zn, Cr and Zr with a purity of 99.99wt.% as raw materials, the melting is carried out in a non-consumable vacuum arc melting furnace in a high-purity argon atmosphere, and repeated 5 times to finally obtain a casting with uniform composition.

[0022] 2. Preparation of room temperature and high temperature tensile specimens: The alloy was rolled at 10% reduction rate per pass in the as-cast state, 50% at room temperature, then solution treated at 1050℃ for 4 hours, water quenched to room temperature, and finally held at 650℃ for 4 hours and then cooled to room temperature in the furnace for aging treatment.

[0023] 3. Preparation of samples for room temperature / high temperature hardness, electrical conductivity and microstructure stability: The ingot was solution treated by holding it at 1050℃ for 4 hours, then water quenched to room temperature, and finally held at 650℃ for 4 hours. It was then cooled to room temperature in the furnace for aging treatment.

[0024] 4. The tissue stability of the aged samples was studied by holding them at 600℃ for 400h.

[0025] Example 2: Alloy Structure and Property Characterization

[0026] 1. The microstructure of the multi-component alloy exhibits good high-temperature stability after prolonged holding at 600℃. Vickers hardness testing of the alloy samples was performed using a Suzhou Maige Instruments HV-1000Z Vickers microhardness tester. The results show that after 400 hours of long-term holding at 600℃, the hardness of the alloy varies within 292±8.8 Hv. (See results below.) Figure 1 As shown in the figure. The hardness change of the alloy during the heating process was tested using the Shandong Zongde Instruments HVZHT-30 high-temperature Vickers hardness testing system. The hardness reached 192Hv at 600℃. The results are as follows. Figure 2 As shown.

[0027] 2. The mechanical properties of the alloy samples were analyzed using a UTM5504 electronic universal testing machine. Room temperature and high temperature tensile tests were conducted according to the national standard GB / T 228.1-2010, "Tension Testing of Metallic Materials at Room Temperature," with a nominal strain rate of 1×10⁻⁶. -4 / s. Based on the obtained stress-strain curves, the various mechanical properties of the material are derived: at room temperature, the tensile strength of the alloy is 819 MPa, and the elongation is 11.1%; at 600℃, the tensile strength is 371 MPa, and the elongation is 3.7%. Figure 3 As shown.

[0028] 3. The room temperature conductivity was measured using a Xiamen Tianyan Sigma2008B eddy current conductivity meter, and the result was 18.4% IACS.

[0029] The above description is merely an embodiment of this application and does not constitute any limitation on this application. Although this application discloses preferred embodiments as described above, it is not intended to limit this application. Any changes or modifications made by those skilled in the art without departing from the scope of the technical solution of this application using the disclosed technical content are equivalent to equivalent implementation cases and fall within the scope of the technical solution.

Claims

1. A high-strength, high-toughness, high-strength, high-toughness Cu-Ni-Al-Cr-Ti-Zr-Zn high-temperature resistant copper alloy with stable microstructure, characterized in that: The copper alloy has the following mass percentage composition: Cu: 83.67~87.67wt%, Ni: 8.55~12.55wt%, Al: 0.81~1.51wt%, Cr: 0.67~1.07wt%, Ti: 0.61~1.01wt%, Zr: 0.32~0.72wt%, Zn: 0.27~0.47wt%. The alloy has an aged room temperature hardness of 297±17.8 Hv, a tensile strength of not less than 819 MPa, an elongation of not less than 11.1%, and an electrical conductivity of not less than 18.4% IACS; at 600℃, the hardness is 192±13.5 Hv, the tensile strength is not less than 371 MPa, and the elongation is not less than 3.7%. After being held at 600℃ for 400 hours, the hardness of the alloy is 292±8.8Hv.

2. The method for preparing a high-strength, high-toughness, high-strength, high-toughness Cu-Ni-Al-Cr-Ti-Zr-Zn high-temperature resistant copper alloy with stable structure according to claim 1, characterized in that, Includes the following steps: The alloy is prepared using high-purity metals of 4N or higher as raw materials; a non-consumable vacuum arc melting furnace is used, and high-purity argon gas is introduced for protection. The raw materials prepared according to the alloy composition in claim 1 according to the mass percentage are repeatedly melted to finally obtain an alloy ingot with uniform composition; then the melted alloy ingot is subjected to solution treatment and aging treatment to obtain a high-strength and high-toughness Cu-Ni-Al-Cr-Ti-Zr-Zn high-temperature resistant copper alloy with stable structure.

3. The preparation method according to claim 2, characterized in that: The solution treatment temperature is 1020℃~1070℃, the time is 3~6h, and then the solution is quenched in water to room temperature.

4. The preparation method according to claim 2, characterized in that: The aging treatment temperature is 600~700℃, the time is 3~6h, and then it is water quenched to room temperature.

5. The preparation method according to claim 2, characterized in that: Cold rolling is performed before solution treatment and aging treatment.

6. The preparation method according to claim 5, characterized in that: The cold rolling process involves reducing the pressure by no more than 20% per pass, with multiple passes until the total pressure reaches 40% to 60%.

Citation Information

Patent Citations

  • Copper alloy and method for producing copper alloy

    CN103328665A

  • Cu-Ni-Al-based copper alloy sheet material, method for producing same, and conductive spring member

    CN115735017A