Modified graphite material, preparation method thereof, negative electrode sheet and application thereof
By introducing carbonyl groups and honeycomb structures onto the surface of graphite materials, combined with ozone treatment, the problems of low specific capacity and poor kinetics of graphite anode materials were solved, resulting in modified graphite materials with high energy density and fast charging performance.
Patent Information
- Application Number
- CN202410524020.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-28
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-04-28
AI Technical Summary
Existing graphite anode materials have low specific capacity and poor kinetics, making it difficult to meet the requirements for high energy density and fast charging performance.
By introducing carbonyl groups and honeycomb structures onto the surface of graphite materials, lithium-ion intercalation sites and diffusion pathways are increased. Ozone treatment is then used to optimize the structure of the graphite materials, resulting in modified graphite materials.
This improves the lithium intercalation capacity and kinetic performance of graphite materials, achieving high energy density and fast charging performance, while also possessing excellent first-time coulombic efficiency and kinetic performance.
Smart Images

Figure CN118439601B_ABST
Abstract
Description
Technical Field
[0001] This application belongs to the field of battery technology, specifically relating to a modified graphite material and its preparation method, a negative electrode sheet, and its application. Background Technology
[0002] Graphite is a layered material where carbon atoms in the same layer form relatively strong covalent bonds through sp2 hybridization, and the layers are bonded together by van der Waals forces. Due to its relatively weak interlayer bonding and large interlayer spacing, it allows for the insertion and extraction of lithium ions, making graphite an important anode material for lithium-ion batteries and an active material for other ion-intercalating electrodes. Currently, high-end graphite has achieved a specific capacity of 360 mAh / g, close to the theoretical specific capacity of 372 mAh / g, but this is insufficient to meet the ever-increasing demands for high energy density. From the perspective of anode materials, improving the energy density of battery cells requires the development of anode materials with even higher specific capacities.
[0003] To address the low specific capacity of graphite anodes, existing technologies employ methods such as preparing single-particle graphite materials with smaller specific surface areas or increasing the graphitization temperature to improve the degree of graphitization, which can enhance the specific capacity of anode graphite to some extent. Single-particle graphite materials with smaller specific surface areas can reduce irreversible lithium consumption during the SEI film formation stage, exhibiting higher initial coulombic efficiency and indirectly improving the specific capacity of graphite. However, these materials have poor kinetics, leading to battery expansion and cell degradation issues during cycling. Increasing the graphitization temperature to improve the degree of graphitization often results in graphite materials with higher initial coulombic efficiency; however, increasing the graphitization temperature requires significant energy consumption, resulting in low return on investment. Furthermore, the reduced interlayer spacing in highly graphitized graphite materials also leads to relatively poorer kinetics. Summary of the Invention
[0004] To address the issues of low specific capacity and poor kinetics in existing negative electrode graphite materials, this application provides a modified graphite material, its preparation method, a negative electrode sheet, and its application. The modified graphite material can increase lithium intercalation sites through carbonyl structure, and the honeycomb structure of the base surface helps to increase lithium ion diffusion paths, thereby simultaneously improving lithium intercalation capacity and kinetics, and obtaining a secondary battery with high energy density and fast charging performance.
[0005] In a first aspect, this application provides a modified graphite material, the base of which has a honeycomb structure, and the infrared spectrum of the modified graphite material contains a characteristic peak of carbonyl groups, the characteristic peak of which is located at 1550 cm⁻¹. -1 Up to 1570cm -1The modified graphite material of this application has carbonyl groups, which can affect the electronic structure and surface properties of graphite, thereby increasing the lithium intercalation sites for adsorbing lithium ions on the basis of the original capacity of graphite. It can increase the lithium intercalation capacity of the modified graphite material without affecting the specific surface area. When combined with the honeycomb structure on the substrate, it is also conducive to increasing the diffusion path of lithium ions and improving the insertion and extraction rates of lithium ions, thereby improving the kinetic performance. Therefore, when used in anode materials, it can give them high energy density and first coulombic efficiency, as well as excellent fast charging performance.
[0006] In some embodiments, the mass content of oxygen on the surface of the modified graphite material (hereinafter referred to as oxygen content) is 0, 0.3% ≤ O ≤ 1.9%. Based on the presence of carbonyl groups in the modified graphite material, this application, when the oxygen content is controlled within the above range, can achieve more lithium intercalation active sites and accelerate the insertion and extraction rates of lithium ions, thereby improving the lithium intercalation capacity and kinetic performance of the modified graphite material.
[0007] Furthermore, modified graphite materials with oxygen content within the range of 1.2% ≤ O ≤ 1.8% can exhibit higher lithium intercalation capacity and kinetic performance.
[0008] In some embodiments, the Id / Ig value in the Raman spectrum of the modified graphite material ranges from 0.119 to 0.155. By controlling the Id / Ig value of the modified graphite material in accordance with the aforementioned carbonyl groups, this application can increase the number of lithium insertion sites and lithium-ion diffusion channels, thereby improving lithium insertion capacity and kinetic performance.
[0009] Furthermore, 0.132≤Id / Ig≤0.151 can achieve even better energy density and kinetic performance.
[0010] In some embodiments, the modified graphite material satisfies at least one of conditions 1 to 5:
[0011] Condition 1: The average particle size d of the modified graphite material is 11.2 μm ≤ d ≤ 24.7 μm.
[0012] Condition 2: The specific surface area (BET) of the modified graphite material is 0.8 m². 2 / g≤BET≤2.2m 2 / g.
[0013] Condition 3: The specific capacity (cpg) of the modified graphite material is 341 mAh / g ≤ cpg ≤ 364 mAh / g.
[0014] Condition 4: The compacted density (cd) of the modified graphite material under 5000 kg pressure is 1.72 g / cm³. 3≤cd≤2.08g / cm 3 .
[0015] Condition 5: The degree of graphitization (gd) of the modified graphite material is 91% ≤ gd ≤ 97%.
[0016] Secondly, this application provides a method for preparing the modified graphite material provided in the first aspect of this application, comprising the following steps: providing graphite; subjecting the graphite to a heat treatment in an ozone-containing atmosphere to obtain the modified graphite material; the heat treatment temperature te is 50℃≤te≤400℃, the heat treatment time ti is 1h≤ti≤10h; and the ozone volume concentration vc in the ozone-containing atmosphere is 2%≤vc≤10%. This application uses ozone to treat graphite, forming additional carbonyl structures for adsorbing lithium ions on the graphite surface, and also optimizes the honeycomb structure of the graphite material's basal surface, thereby increasing the lithium intercalation capacity and diffusion path of the modified graphite material, and improving its energy density and kinetic performance.
[0017] In some embodiments, the graphite is selected from synthetic graphite and / or natural graphite.
[0018] In some embodiments, the temperature te for the heat preservation treatment is 110℃≤te≤350℃, and the time ti is 2h≤ti≤5h. Under these conditions, the heat preservation treatment can further optimize the number of carbonyl groups and the honeycomb structure on the graphite surface, achieving higher lithium intercalation capacity and kinetic performance.
[0019] In some embodiments, the volume concentration vc of ozone in the ozone-containing atmosphere is 5% ≤ vc ≤ 8%. Controlling the volume concentration of ozone in the ozone-containing atmosphere within this preferred range allows for better treatment of defect structures on the graphite surface, thereby improving the lithium intercalation capacity and rate performance of the modified graphite material.
[0020] In some embodiments, the volumetric flow rate vfr of the ozone-containing atmosphere is 500 mL / min ≤ vfr ≤ 3000 mL / min.
[0021] Thirdly, this application provides a negative electrode sheet, comprising the modified graphite material provided in the first aspect of this application or the modified graphite material prepared by the preparation method provided in the second aspect. Because the negative electrode sheet of this application comprises the modified graphite material provided in this application, it possesses the same advantages, achieving higher energy density and first coulombic efficiency, while also exhibiting excellent kinetic performance.
[0022] In some embodiments, the water contact angle (hereinafter referred to as the electrode contact angle) θ of the negative electrode at 25°C is 82°≤θ≤110°; preferably, 82°≤θ≤88°. The modified graphite material of this application has high hydrophilicity and strong polarity due to the presence of carbonyl groups. Therefore, when applied to the electrode, it can achieve a low water contact angle, which is beneficial to improving the compatibility and wettability of the modified graphite material with the electrolyte, reducing electrode polarization and charge transfer resistance, thereby further improving the kinetic performance of the electrode.
[0023] Fourthly, this application provides a secondary battery that includes the negative electrode sheet provided in the third aspect of this application. Because the secondary battery provided by this application includes the aforementioned negative electrode sheet, it achieves the same advantages, exhibiting excellent energy density and kinetic performance, as well as excellent fast-charging performance.
[0024] Fifthly, an electronic device includes the secondary battery provided in the fourth aspect of this application. Because the electronic device of this application includes the aforementioned secondary battery, it can achieve the same advantages, possessing excellent battery life and fast charging performance, thus having high application prospects.
[0025] The modified graphite material, its preparation method, negative electrode sheet, and applications based on this application have at least the following beneficial effects:
[0026] 1. By modifying the carbonyl groups on the graphite surface to increase additional lithium ion insertion sites, and in combination with the honeycomb structure on the substrate, it is also beneficial to increase the insertion and extraction rates of lithium ions, thereby improving the lithium insertion capacity and kinetic performance.
[0027] 2. Using ozone to treat graphite optimizes the structure of modified graphite materials, which can improve their energy density and kinetic performance. At the same time, it does not have an adverse effect on the specific surface area and initial coulombic efficiency of graphite materials. It also has the advantages of simple process, convenient operation, low cost, and easy promotion and mass production.
[0028] 3. When the modified graphite material of this application is used in anode materials, secondary batteries and electronic devices, it can give it high energy density and first coulombic efficiency, as well as excellent fast charging performance. Attached Figure Description
[0029] Figure 1 The images show the scanning tunneling microscope morphology of the basal surface of the modified graphite materials provided in Examples 1-22 of this application.
[0030] Figure 2 Infrared spectra of the modified graphite materials provided in Examples 1-22 of this application and the graphite material of Comparative Example 1;
[0031] Figure 3 Electrochemical impedance spectroscopy of the modified graphite materials of Examples 1-22 and the graphite material of Comparative Example 1;
[0032] Figure 4 The charging and discharging capacity test data of coin lithium-ion batteries prepared from the modified graphite materials of Examples 1-22 and the graphite material of Comparative Example 1. Detailed Implementation
[0033] To make the objectives, technical solutions, and advantages of this application clearer, the following detailed description is provided in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the scope of this application.
[0034] In their research on improving the specific capacity of graphite, the inventors discovered that in practical applications, graphite needs to maintain its intrinsic layered structure and have a relatively large micron-sized particle size. This results in slow diffusion kinetics of ions intercalating and deintercalating between graphite layers, leading to poor rate performance of the graphite anode and easy lithium plating during high-rate charging. To address the poor kinetics of graphite anodes, a layer of disordered amorphous carbon is coated onto the graphite surface to provide more diffusion channels, which can improve the kinetic performance of the graphite anode to some extent. However, coating the graphite surface with amorphous carbon reduces the initial efficiency, thereby lowering the cell's energy density.
[0035] In view of this, this application proposes a modified graphite material, wherein the basal surface of the modified graphite material has a honeycomb structure, and the infrared spectrum of the modified graphite material has a characteristic peak of carbonyl group, the characteristic peak of carbonyl group being located at 1550 cm⁻¹. -1 Up to 1570cm -1 By introducing carbonyl groups into modified graphite materials and combining them with honeycomb structures on the substrate, the carbon defect structures on the graphite surface that do not contribute to capacity can be utilized, providing lithium intercalation sites and lithium-ion diffusion pathways to increase capacity. This improves the lithium intercalation capacity and kinetic performance of the modified graphite materials, enabling secondary batteries to have high energy density and high kinetic performance, as well as rate performance and fast charging performance.
[0036] In this application, in the crystal structure of graphite, the surface between layers is called the basal plane (0001), and the rectangular side surface perpendicular to the basal plane is called the prism (1010). The honeycomb structure refers to the modified graphite material of this application having multiple repeating polygonal units in its basal plane, wherein adjacent polygonal units are connected to each other by sharing adjacent edges and are arranged in an orderly manner, similar to the honeycomb structure in nature. The polygonal units in this application include, but are not limited to, hexagons.
[0037] In some exemplary embodiments, the oxygen content on the surface of the modified graphite material is O, with a mass content of 0.3% ≤ O ≤ 1.9%. For example, O is selected from 0.3%, 0.5%, 0.7%, 0.8%, 1.0%, 1.2%, 1.3%, 1.5%, 1.7%, 1.8%, or any two of the above values. In some more preferred embodiments, 1.2% ≤ O ≤ 1.8%. Based on the presence of carbonyl groups in the modified graphite material, this application uses the oxygen content to reflect the carbonyl content in the modified graphite material. When the oxygen content is controlled within the above range, the modified graphite material can have more lithium intercalation active sites, thereby improving the lithium intercalation capacity of the modified graphite material. Simultaneously, a suitable oxygen content in the modified graphite material can also accelerate the lithium ion insertion and extraction rate, optimizing the kinetic performance of the modified graphite material.
[0038] It should be noted that, unlike the abstract "surface" in mathematical geometry, in the field of physical chemistry, the "surface" of an object is a physical layer with a physical form. In this case, the surface of a solid refers to the solid-gas interface or solid-liquid interface layer, which is actually a physical layer composed of one or several atomic layers of condensed matter close to a gas or vacuum.
[0039] In some embodiments, the mass percentage of oxygen on the surface of the modified graphite material was measured using X-ray photoelectron spectroscopy (XPS).
[0040] It is understandable that when the mass percentage of oxygen on the surface of modified graphite is measured using an X-ray photoelectron spectroscopy (XPS), the result detected by the XPS is the content of oxygen on the surface of the modified graphite. At this time, the surface of the modified graphite is the part that X-rays pass through and detect during the XPS test.
[0041] Specifically, X-ray photoelectron spectroscopy (XPS) is a technique for analyzing the chemical properties of a material's surface. It utilizes the absorption and scattering characteristics of X-rays as they pass through an object's surface to detect its internal structure. XPS can measure the elemental composition, empirical formulas, chemical states, and electronic states of elements in materials. It involves exciting a solid surface with a beam of X-rays and simultaneously measuring the kinetic energy of electrons emitted from the surface of the analyzed material within a range of 1–10 nm to obtain the XPS spectrum. Photoelectron spectroscopy records electrons with energies exceeding a certain threshold. The spectral peaks appearing in the photoelectron spectrum represent the emission of electrons with specific energies from atoms. The energy and intensity of these peaks can be used for qualitative and quantitative analysis of the elements contained in a solid surface.
[0042] In some exemplary embodiments, the Id / Ig value in the Raman spectrum of the modified graphite material ranges from 0.119 to 0.155. For example, Id / Ig is selected from 0.119, 0.123, 0.127, 0.130, 0.132, 0.136, 0.138, 0.144, 0.147, 0.151, 0.153, 0.155, or any two of the above values. In some more preferred embodiments, the Id / Ig value in the Raman spectrum of the modified graphite material is 0.132 to 0.151. This application controls the Id / Ig value of the modified graphite material to coordinate with the carbonyl groups mentioned above. By utilizing the disordered structure in the modified graphite material, more lithium intercalation sites can be added, more lithium-ion diffusion channels can be provided, and the diffusion barrier can be reduced, thereby improving the lithium intercalation capacity and kinetic performance.
[0043] In some exemplary embodiments, the average particle size d of the modified graphite material is 11.2 μm ≤ d ≤ 24.7 μm. For example, the average particle size d of the modified graphite material can be selected from 11.2 μm, 12.7 μm, 14.4 μm, 15.4 μm, 17.4 μm, 18.8 μm, 20.2 μm, 21.1 μm, 22.1 μm, 24.0 μm, 24.7 μm, or any two of the above values. Modified graphite materials with the above average particle size are advantageous for obtaining shorter lithium-ion diffusion paths, thereby further improving the kinetic performance of secondary batteries.
[0044] In some exemplary embodiments, the specific surface area (BET) of the modified graphite material is 0.8 m². 2 / g≤BET≤2.2m 2 / g. For example, the specific surface area BET of the modified graphite material is selected from 0.8m². 2 / g, 1.0m 2 / g, 1.1m 2 / g, 1.3m 2 / g, 1.4m 2 / g, 1.5m 2 / g, 1.8m 2 / g, 1.9m 2 / g、2.1m 2 / g, 2.2m 2 / g or any two of the above values. By controlling the specific surface area of the modified graphite material within the above range, it can have more active sites for lithium ion intercalation, thereby achieving a higher lithium intercalation capacity.
[0045] In some exemplary embodiments, the specific capacity (cpg) of the modified graphite material is 341 mAh / g ≤ cpg ≤ 364 mAh / g. For example, the specific capacity (cpg) of the modified graphite material is selected from 341 mAh / g, 343 mAh / g, 346 mAh / g, 349 mAh / g, 351 mAh / g, 355 mAh / g, 355 mAh / g, 359 mAh / g, 362 mAh / g, 364 mAh / g, or any two of the above values. By controlling the specific capacity of the modified graphite material within the above range, the lithium-ion diffusion path and lithium intercalation capability can be further balanced and optimized, achieving higher capacity and kinetic performance, thereby improving the first coulombic efficiency and rate performance of the secondary battery.
[0046] In some exemplary embodiments, the compaction density (cd) of the modified graphite material under 5000 kg pressure is 1.72 g / cm³. 3 ≤cd≤2.08g / cm 3 For example, the compaction density (cd) of modified graphite material under 5000 kg pressure is selected from 1.72 g / cm³. 3 1.76 g / cm 3 1.81 g / cm 3 1.84 g / cm 3 1.87 g / cm 3 1.91g / cm 3 1.97g / cm 3 2.02 g / cm 3 2.06 g / cm 3 2.08 g / cm 3 Or any two of the above values within a range. Modified graphite materials with a compaction density within the above range can fully utilize the gaps between particles, improve lithium intercalation capacity and lithium-ion diffusion pathways, and further improve the lithium intercalation capacity and kinetic performance of secondary batteries.
[0047] In some exemplary embodiments, the degree of graphitization (gd) of the modified graphite material is 91% ≤ gd ≤ 97%. For example, the degree of graphitization (gd) of the modified graphite material is selected from 91%, 92%, 93%, 94%, 95%, 96%, 97%, or any two of the above values. By controlling the degree of graphitization of the modified graphite material within the above range, this application can further optimize the intercalation and diffusion behavior of lithium ions in the modified graphite material, thereby improving the lithium intercalation capacity and kinetic performance.
[0048] Secondly, this application provides a method for preparing the modified graphite material provided in the first aspect of this application, comprising the following steps: providing graphite; subjecting the graphite to heat treatment in an ozone-containing atmosphere to obtain the modified graphite material; the heat treatment temperature te is 50℃≤te≤400℃, the heat treatment time ti is 1h≤ti≤10h; and the ozone volume concentration vc in the ozone-containing atmosphere is 2%≤vc≤10%. This application uses ozone to treat graphite, utilizing the highly reactive oxygen free radicals O* generated by ozone decomposition to react with the non-capacitating carbon defect structures on the graphite surface, forming additional carbonyl structures for adsorbing lithium ions on the graphite surface. This generates lithium intercalation sites that increase capacity and optimizes the honeycomb structure of the graphite material's basal surface, thereby increasing the lithium intercalation capacity and diffusion path of the modified graphite material, improving its energy density and kinetic performance, while not adversely affecting the specific surface area and initial coulombic efficiency of the graphite material. This method also has the advantages of simple process, convenient operation, and low cost.
[0049] In some exemplary embodiments, the graphite is selected from synthetic graphite and / or natural graphite. The graphite material in this application may be selected from at least one of natural graphite, uncoated synthetic graphite, or synthetic graphite coated with amorphous carbon.
[0050] In this application, the source of the ozone-containing atmosphere is not specifically limited, as long as the volume concentration of ozone mentioned above is met. For example, the ozone-containing atmosphere can be prepared by reacting ultraviolet light, corona discharge, or plasma with oxygen-containing gas, such as using an ultraviolet lamp or an ozone generator. The wavelength range of the ultraviolet lamp is 150–400 nm, for example, it can be 150 nm, 160 nm, 170 nm, 180 nm, 190 nm, 200 nm, 210 nm, 220 nm, 230 nm, 240 nm, 250 nm, 260 nm, 270 nm, 280 nm, 290 nm, 300 nm, 310 nm, 320 nm, 330 nm, 340 nm, 350 nm, 360 nm, 370 nm, 380 nm, 390 nm, 400 nm, or any combination of two of the above values.
[0051] In some embodiments of this application, the heat preservation treatment can keep the graphite in a tumbling and dispersed state during the treatment process so that it can fully contact the ozone. For example, at least one of the treatment equipment such as a rotary kiln or a fluidized bed can be used to keep the graphite in a tumbling and dispersed state, thereby increasing the contact area between the graphite and the ozone.
[0052] In some exemplary embodiments, the rotational speed of the processing device can be from 1 to 12 rad / s, for example, it can be 1 rad / s, 2 rad / s, 3 rad / s, 4 rad / s, 5 rad / s, 6 rad / s, 7 rad / s, 8 rad / s, 9 rad / s, 10 rad / s, 11 rad / s, 12 rad / s or any two of the above values.
[0053] In some exemplary embodiments, the power of the ultraviolet lamp or ozone generator is 50 to 10000W, for example, it can be 50W, 100W, 500W, 1000W, 2000W, 3000W, 4000W, 5000W, 6000W, 7000W, 8000W, 9000W, 10000W or any combination of two of the above values.
[0054] In some exemplary embodiments, the temperature te of the heat preservation treatment is 50℃≤te≤400℃, preferably, the temperature te of the heat preservation treatment is 110℃≤te≤350℃. Exemplarily, the temperature te of the heat preservation treatment is selected from 50℃, 89℃, 110℃, 131℃, 150℃, 157℃, 200℃, 204℃, 234℃, 250℃, 274℃, 300℃, 317℃, 350℃, 377℃, 400℃, or any two of the above values.
[0055] In some exemplary embodiments, the heat preservation time ti is 1h ≤ ti ≤ 10h, preferably 2h ≤ ti ≤ 5h. Exemplarily, the heat preservation time ti is selected from 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h or any two of the above values.
[0056] Performing heat preservation treatment under the above temperature and time range is beneficial to optimizing the number of carbonyl groups and honeycomb structure on the graphite surface, thereby improving lithium intercalation capacity and kinetic performance.
[0057] In some exemplary embodiments, the heating process to the holding temperature can be carried out under the protection of an inert gas (such as nitrogen) at a flow rate of 1000 mL / min, heating from room temperature of 25°C to 100°C in 60 minutes. In some exemplary embodiments, the volume concentration vc of ozone in the ozone-containing atmosphere is 2% ≤ vc ≤ 10%, for example, the volume concentration vc of ozone in the ozone-containing atmosphere is selected from 2%, 3%, 4%, 5%, 6%, 7%, 8%, 9%, 10%, or any two of the above values. Preferably, the volume concentration vc of ozone in the ozone-containing atmosphere is 5% ≤ vc ≤ 8%. When the volume concentration of ozone in the ozone-containing atmosphere is controlled within the above range, it is beneficial to optimize the defect structure of the graphite surface and improve the lithium intercalation capacity and kinetic performance of the modified graphite material.
[0058] In some exemplary embodiments, the volumetric flow rate (vfr) of the ozone-containing atmosphere is 500 mL / min ≤ vfr ≤ 3000 mL / min. For example, the volumetric flow rate (vfr) of the ozone-containing atmosphere is selected from 500 mL / min, 790 mL / min, 1076 mL / min, 1299 mL / min, 1515 mL / min, 1902 mL / min, 2246 mL / min, 2463 mL / min, 2728 mL / min, 2936 mL / min, 3000 mL / min, or any two of the above values. By controlling the volumetric flow rate of the ozone-containing atmosphere within the above range, this application can further promote the reaction process between ozone and graphite raw materials, and optimize the energy density and kinetics of the modified graphite material.
[0059] This application does not impose any particular restrictions on the methods for controlling the oxygen content and Id / Ig ratio of the modified graphite material, as long as the purpose of this application can be achieved. Generally, the oxygen content and Id / Ig ratio of the modified graphite material can be controlled by adjusting the process conditions in the preparation method of this application. For example, the oxygen content and Id / Ig ratio of the modified graphite material can be controlled by changing the temperature and holding time of the heat treatment, the rotation speed of the processing equipment, the volume concentration of ozone in the ozone-containing atmosphere, and the volumetric flow rate of the ozone-containing atmosphere, thereby controlling the various properties of the modified graphite material of this application.
[0060] Thirdly, this application provides a negative electrode sheet, including the modified graphite material provided in the first aspect of this application or the modified graphite material prepared by the preparation method provided in the second aspect.
[0061] In some exemplary embodiments, the water contact angle θ of the negative electrode at 25°C is 82°≤θ≤110°; preferably, 82°≤θ≤88°. Exemplarily, the water contact angle θ of the negative electrode at 25°C is selected from 82°, 85°, 88°, 92°, 94°, 98°, 99°, 102°, 107°, 108°, 110°, or any two of the above values.
[0062] By adjusting the above-mentioned process conditions in the preparation method of the modified graphite material of this application, the water contact angle of the negative electrode sheet at 25°C can be controlled.
[0063] In this application, modified graphite material is included as the negative electrode material in the negative electrode flux layer of the negative electrode sheet. The negative electrode sheet of this application also includes a negative electrode current collector. In this application, the negative electrode flux layer can be disposed on one surface in the thickness direction of the negative electrode current collector, or on both surfaces in the thickness direction of the negative electrode current collector. It should be noted that "surface" here can refer to the entire area of the negative electrode current collector or only a portion thereof; this application has no particular limitation, as long as the purpose of this application is achieved. This application has no particular limitation on the thickness of the negative electrode flux layer, as long as the purpose of this application is achieved. For example, the thickness of a single-sided negative electrode flux layer can be from 30 μm to 160 μm.
[0064] This application does not impose any particular limitation on the negative electrode current collector, as long as it achieves the purpose of this application. For example, the negative electrode current collector may include copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, or composite current collectors (e.g., carbon-copper composite current collector, nickel-copper composite current collector, titanium-copper composite current collector), etc. This application does not impose any particular limitation on the thickness of the negative electrode current collector, as long as it achieves the purpose of this application. For example, the thickness of the negative electrode current collector may be from 4 μm to 10 μm.
[0065] In this application, the negative electrode binder may also be included in the negative electrode binder layer. This application does not have any particular limitation on the negative electrode binder, as long as it can achieve the purpose of this application. For example, it may include, but is not limited to, at least one of polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyacrylic acid, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin or nylon.
[0066] In this application, the negative electrode binder layer may further include a conductive agent. This application does not impose any particular limitation on the type of conductive agent in the negative electrode binder layer, as long as it achieves the purpose of this application. For example, the conductive agent may include, but is not limited to, at least one of conductive carbon black (Super P), carbon nanotubes (CNTs), carbon fibers, flake graphite, Ketjen black, graphene, metallic materials, or conductive polymers. The aforementioned carbon nanotubes may include, but are not limited to, single-walled carbon nanotubes and / or multi-walled carbon nanotubes. The aforementioned carbon fibers may include, but are not limited to, vapor-grown carbon fibers (VGCF) and / or carbon nanofibers. The aforementioned metallic materials may include, but are not limited to, metal powders and / or metal fibers; specifically, the metal may include, but is not limited to, at least one of copper, nickel, aluminum, or silver. The aforementioned conductive polymer may include, but is not limited to, at least one of polyphenylene derivatives, polyaniline, polythiophene, polyacetylene, or polypyrrole. This application does not impose any particular limitation on the mass ratio of the negative electrode material, conductive agent, and negative electrode binder in the negative electrode binder layer, as long as it achieves the purpose of this application.
[0067] Fourthly, this application provides a secondary battery, which includes the negative electrode provided in the third aspect of this application.
[0068] The secondary battery described in this application is not particularly limited and may include any device in which an electrochemical reaction occurs. In one embodiment of this application, the secondary battery may include, but is not limited to, lithium-ion secondary batteries (lithium-ion batteries), sodium-ion batteries, lithium polymer secondary batteries, or lithium-ion polymer secondary batteries.
[0069] In some exemplary embodiments of this application, the secondary battery further includes a positive electrode, an electrolyte, and a separator.
[0070] This application does not impose any particular limitation on the positive electrode sheet, as long as the purpose of this application can be achieved. For example, the positive electrode sheet includes a positive current collector and a positive electrode additive layer located on at least one surface of the positive current collector. The aforementioned "positive electrode additive layer located on at least one surface of the positive current collector" means that the positive electrode additive layer can be located on one surface of the positive current collector along its own thickness direction, or it can be located on two surfaces of the positive current collector along its own thickness direction. It should be noted that the "surface" here can be the entire surface area of the positive current collector, or it can be a partial surface area of the positive current collector; this application does not impose any particular limitation, as long as the purpose of this application can be achieved.
[0071] This application does not impose any particular restrictions on the positive electrode current collector, as long as it can achieve the purpose of this application. For example, the positive electrode current collector may include aluminum foil, aluminum alloy foil, or composite current collectors (such as aluminum-carbon composite current collectors).
[0072] The positive electrode mixture layer of this application includes a positive electrode material. This application does not particularly limit the type of positive electrode material, as long as it can achieve the purpose of this application. For example, the positive electrode material may include lithium nickel cobalt manganese oxide (LiNi). 0.90 Co 0.05 Mn 0.05 At least one of the following: O2 (NCM955), NCM811, NCM622, NCM523, NCM111, lithium nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich manganese-based materials, lithium cobalt oxide (LiCoO2), lithium manganese oxide, lithium manganese iron phosphate, or lithium titanate. In this application, the cathode material may also contain non-metallic elements, such as at least one of fluorine, phosphorus, boron, chlorine, silicon, or sulfur. In this application, there are no particular limitations on the thickness of the cathode current collector and the cathode flux layer, as long as the purpose of this application is achieved. For example, the thickness of the cathode current collector is 5 μm to 20 μm, and the thickness of the single-sided cathode flux layer is 30 μm to 120 μm.
[0073] In this application, the positive electrode binder layer may further include a positive electrode binder and a conductive agent. This application does not impose any particular limitation on the type of positive electrode binder in the positive electrode binder layer, as long as it can achieve the purpose of this application. For example, the positive electrode binder may include, but is not limited to, at least one of polyvinylidene fluoride, polytetrafluoroethylene, polyolefins, sodium carboxymethyl cellulose, lithium carboxymethyl cellulose, modified polyvinylidene fluoride, modified styrene-butadiene rubber (SBR), or polyurethane.
[0074] This application does not impose any particular restrictions on the type of conductive agent in the positive electrode binder layer, as long as it achieves the purpose of this application. For example, the conductive agent can be the same type as the conductive agent in the negative electrode binder layer. This application does not impose any particular restrictions on the mass ratio of positive electrode material, conductive agent, and positive electrode binder in the positive electrode binder layer. Those skilled in the art can select according to actual needs, as long as the purpose of this application is achieved.
[0075] In this application, the electrolyte includes lithium salts and non-aqueous solvents. The lithium salt may include at least one of LiPF6, LiPO2F2, LiNO3, LiBF4, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, Li2SiF6, lithium bis(oxalato)borate (LiBOB), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), or lithium difluoroborate. This application does not limit the content of lithium salts in the electrolyte, as long as the purpose of this application is achieved. This application does not particularly limit the non-aqueous solvent, as long as the purpose of this application is achieved. For example, the non-aqueous solvent may include, but is not limited to, at least one of carbonate compounds, carboxylic acid ester compounds, ether compounds, or other organic solvents. The aforementioned carbonate compounds may include, but are not limited to, at least one of chain carbonate compounds, cyclic carbonate compounds, or fluorocarbonate compounds. The aforementioned chain carbonate compounds may include, but are not limited to, at least one of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, or methyl ethyl carbonate. The aforementioned cyclic carbonates may include, but are not limited to, at least one of ethylene carbonate, propylene carbonate (PC), butylene carbonate, or vinylene carbonate. Fluorinated carbonate compounds may include, but are not limited to, at least one of fluoroethylene carbonate, 1,2-difluoroethylene carbonate, 1,1,2-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, or trifluoromethylethylene carbonate. The aforementioned carboxylic acid ester compounds may include, but are not limited to, at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanolactone, valproic acid lactone, or caprolactone. The aforementioned ether compounds may include, but are not limited to, at least one of dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran, or tetrahydrofuran. The aforementioned other organic solvents may include, but are not limited to, at least one of dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolium ketone, N-methyl-2-pyrrolidone, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate, or trioctyl phosphate.
[0076] The secondary battery of this application also includes a separator. This application does not impose any particular limitation on the separator, as long as it achieves the purpose of this application. For example, the material of the separator can include, but is not limited to, at least one of polyethylene (PE), polypropylene (PP), polyolefin (PO) separators based on polytetrafluoroethylene, polyester films (e.g., polyethylene terephthalate (PET) films), cellulose films, polyimide films (PI), polyamide films (PA), spandex, or aramid films. The type of separator can include, but is not limited to, at least one of woven films, nonwoven films (non-woven fabrics), microporous films, composite films, rolled films, or spun films. The separator of this application can have a porous structure, and the pore size is not particularly limited, as long as it achieves the purpose of this application. For example, the pore size can be from 0.01 μm to 1 μm. In this application, the thickness of the separator is not particularly limited, as long as it achieves the purpose of this application. For example, the thickness can be from 5 μm to 500 μm.
[0077] The secondary battery of this application also includes a packaging bag for containing the positive electrode, negative electrode, separator, and electrolyte, as well as other components known in the art for secondary batteries. This application does not limit the aforementioned other components. This application does not impose any particular limitation on the packaging bag; it can be any packaging bag known in the art, as long as it can achieve the purpose of this application.
[0078] The preparation process of the secondary battery described in this application is well known to those skilled in the art, and this application has no particular limitations. For example, it may include, but is not limited to, the following steps: stacking the positive electrode, separator, and negative electrode in sequence, and performing operations such as winding and folding as needed to obtain a wound electrode assembly; placing the electrode assembly in a packaging bag; injecting electrolyte into the packaging bag and sealing it to obtain a secondary battery; or stacking the positive electrode, separator, and negative electrode in sequence, and then fixing the four corners of the entire stacked structure with tape to obtain a stacked electrode assembly; placing the electrode assembly in a packaging bag; injecting electrolyte into the packaging bag and sealing it to obtain a secondary battery. In addition, overcurrent protection components, conductive plates, etc., may be placed in the packaging bag as needed to prevent the internal pressure of the secondary battery from rising and overcharging / discharging.
[0079] Fifthly, this application provides an electronic device that includes the secondary battery provided in the fourth aspect of this application.
[0080] The electronic device described in this application is not particularly limited and can be any electronic device known in the prior art. For example, the electronic device may include, but is not limited to, laptops, pen input computers, mobile computers, e-book players, portable telephones, portable fax machines, portable copiers, portable printers, stereo headphones, video recorders, LCD TVs, portable cleaners, portable CD players, mini CDs, transceivers, electronic notebooks, calculators, memory cards, portable recorders, radios, backup power supplies, motors, automobiles, motorcycles, electric bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, household large-capacity batteries, and lithium-ion capacitors.
[0081] The following specific embodiments illustrate the solution of this application. Unless otherwise specified, the raw materials used in the following embodiments are all from commercially available products, and the apparatus or equipment used are all purchased from conventional market sales channels. Various tests and evaluations were conducted according to the methods described below. Furthermore, unless otherwise specified, "parts" and "%" are quality standards.
[0082] Example 1
[0083] This embodiment provides a modified graphite material whose basal structure can be characterized by scanning tunneling microscopy using a Bruker (formerly Veeco) microscope to reveal a honeycomb structure on the basal surface.
[0084] The modified graphite material exhibits a characteristic peak of carbonyl groups in its infrared spectrum, with the carbonyl group characteristic peak located at 1550 cm⁻¹. -1 Up to 1570cm -1 The infrared spectroscopy of modified graphite materials can be performed using a JASCO FTIR-430 advanced Fourier transform infrared spectrometer. Before the infrared spectroscopy test, the modified graphite material sample is dried at 60℃ for 5 hours, and the sample is pressed into a potassium bromide pellet. The measurement is performed in transmission mode.
[0085] The oxygen content of the modified graphite material can be tested using methods known in the art. For example, the oxygen content of the modified graphite material sample can be quantitatively tested using a Shimadzu / Kratos AXIS SUPRA+ X-ray photoelectron spectroscopy system. In this embodiment, the oxygen content (O) of the modified graphite material is 0.5%.
[0086] The Id / Ig ratio of modified graphite materials can be obtained by scanning the modified graphite sample using a laser confocal Raman spectrometer (Raman, HREvolution, HORIBA Scientific Instruments Division). This allows for the acquisition of the d and g peaks of all sample particles within the specified area. The data is then processed using LabSpec software to obtain the peak intensities of the d and g peaks for each sample particle, denoted as Id and Ig, respectively. The frequency of Id / Ig is statistically analyzed in steps of 0.02 to obtain a normal distribution. The (Id / Ig)max and (Id / Ig)min values for these sample particles are then calculated, and the average Id / Ig value is obtained, representing the Id / Ig value of the modified graphite material. The laser wavelength of the Raman spectrometer can be in the range of 532 nm to 785 nm. The d-peak is located near 1350 cm⁻¹ and is caused by the radial breathing mode of the symmetric stretching vibration of sp² carbon atoms in the aromatic ring (i.e., structural defects); the g-peak appears near 1580 cm⁻¹ and is caused by the stretching vibration between sp² carbon atoms, which corresponds to the vibration of the E²g optical phonon at the center of the Brillouin zone (i.e., in-plane vibration of carbon atoms). In this embodiment, the modified graphite material has an Id / Ig ratio of 0.1194.
[0087] The average particle size of the modified graphite material can be tested using methods known in the art. For example, a laser diffraction particle size distribution measuring instrument (Malvem Mastersizer 3000) can be used to measure the particle size distribution of the modified graphite material sample according to the particle size distribution laser diffraction method GB / T19077-2016, thereby obtaining the average particle size of the corresponding modified graphite material. Alternatively, a sample area can be selected on the negative electrode sheet, and a SEM image of the sample area can be obtained. The average particle size of the modified graphite material can be calculated based on the particle size of the modified graphite material sample in the SEM image. In this embodiment, the average particle size of the modified graphite material is d = 13 μm.
[0088] The specific surface area of modified graphite materials can be tested using methods known in the art, such as the nitrogen adsorption specific surface area analysis method according to GB / T19587-2017, and calculated using the BET (Brunauer Emmett Teller) method. For example, the process may include the following steps: pretreating a modified graphite material sample at 200°C under a nitrogen atmosphere for 2 hours to remove impurities adsorbed on the material surface; then adsorbing the sample with nitrogen as the adsorbate in a liquid nitrogen environment; and finally calculating the specific surface area of the corresponding material using the BET method after adsorption saturation. In this embodiment, the specific surface area of the modified graphite material is BET = 1.0 m². 2 / g.
[0089] The specific capacity test of the modified graphite material includes the following steps: A coin cell is placed on a blue battery tester for testing. The test procedure is as follows: Step 1: Discharge at 0.05C to 0V; Step 2: Rest for 5 minutes; Step 3: Discharge at 50μA to 0V; Step 4: Rest for 5 minutes; Step 5: Discharge at 20μA to 0V; Step 6: Rest for 5 minutes; Step 7: Charge at 0.1C to 2V; Step 8: Rest for 5 minutes. Steps 1 to 8 are repeated twice. Then, the battery is discharged at 1C to 0V, rested for 5 minutes, and charged at 0.1C to 2V, ending the test. The cumulative capacity of the three discharge stages (steps 1, 3, and 5) in the first cycle is the discharge capacity. Charging at 0.1C to 2.0V yields the charging capacity. Dividing the charging capacity by the weight of the modified graphite material gives the specific capacity of the modified graphite material. Dividing the charging capacity by the discharge capacity gives the initial coulombic efficiency. In this embodiment, the specific capacity of the modified graphite material is cpg = 358.6 mAh / g.
[0090] The compaction density test of modified graphite materials under 5000 kg pressure can be performed according to the national standard GB / T24533-2009 "Graphite Anode Materials for Lithium-ion Batteries". The specific test method includes: weighing 1.0000±0.0500 g of modified graphite material sample and placing it in a test mold (model: CARVER#361913mm). Then, the sample is placed in the testing equipment (Sansi Zongheng UTM7305), with a testing capacity of 5 tons (5000 kg), a pressure increase rate of 10 mm / min, a pressure holding time of 30 s, a pressure release rate of 30 mm / min, and a pressure release holding time of 10 s. The formula for calculating the compaction density is: Compaction density = Material mass / (Material bearing area × Sample thickness), unit: g / cm³. 3 The modified graphite material provided in this embodiment has a compaction density (cd) of 1.97 g / cm³ under a pressure of 5000 kg. 3 .
[0091] The degree of graphitization of the modified graphite material was tested using methods known in the art. For example, a method including the following steps could be used: using high-purity silicon powder as a standard, the modified graphite material sample and the silicon standard were mixed at a weight ratio of 5:1. The 002 peak of the sample and the 111 peak of silicon were obtained. The obtained graphite 002 peak was calibrated, and the degree of graphitization was indirectly calculated using the calibrated 002 interplanar spacing d002. The calculation formula is g = (0.344 - d002) / (0.344 - 0.3354), where 0.3440 represents the interlayer spacing of completely ungraphitized carbon, and 0.3354 represents the interlayer spacing of ideal graphite, both in nm. In this embodiment, the degree of graphitization of the modified graphite material is gd = 95.2%.
[0092] The modified graphite material in this embodiment is prepared using a method comprising the following steps:
[0093] Using artificial graphite as raw material, 100g was placed in a rotary kiln with a rotation speed of 1 rad / s. Under a nitrogen protective gas atmosphere, the nitrogen flow rate was 1000 mL / min, and the temperature was raised from room temperature (25°C) to 100°C over 60 minutes. Using 99.999% high-purity oxygen as the gas source, ozone was produced using a 100g / h ozone generator manufactured by Xuzhou Tianlan Ozone Equipment Co., Ltd. The ozone volume concentration in the ozone-containing atmosphere was 5%, and the ozone volume flow rate was 1500 mL / min. The mixture was held at 100°C for 1 hour. After the holding period, under a nitrogen protective gas atmosphere with a nitrogen flow rate of 1000 mL / min, the mixture was naturally cooled to room temperature, yielding the modified graphite material of this embodiment.
[0094] The preparation method of the negative electrode sheet specifically includes the following steps:
[0095] Modified graphite material was used as the negative electrode material and dispersed evenly with sodium carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) in an appropriate amount of deionized water at a mass ratio of 97.5:1.2:1.3 to obtain a negative electrode slurry. Using copper foil as the current collector, the negative electrode slurry was uniformly coated onto the current collector. After coating, it was dried and cold-pressed to obtain the negative electrode sheet.
[0096] The water contact angle of the negative electrode at 25°C can be tested using methods known in the art. For example, at 25°C, a contact angle tester (such as SDC200S) can be used to measure the water contact angle: a water droplet of 10μL±1μL is dropped onto the surface of the negative electrode, and the water contact angle is measured 35 seconds after the water droplet is dropped. Specifically, the water contact angle is measured by the average value of the angles on the left and right sides of the droplet, and the specific value is automatically fitted and read by the instrument.
[0097] In this embodiment, the water contact angle θ of the negative electrode at 25°C is 110°.
[0098] The preparation method of the positive electrode sheet specifically includes the following steps:
[0099] Lithium cobalt oxide (chemical formula: LiCoO2) is used as the positive electrode material. It is mixed with conductive agent acetylene black and binder polyvinylidene fluoride (PVDF) in a weight ratio of 96.3:2.2:1.5 in an appropriate amount of N-methylpyrrolidone (NMP) solvent to form a uniform positive electrode slurry. The positive electrode slurry is coated onto current collector aluminum foil, dried and cold-pressed after coating to obtain the positive electrode sheet.
[0100] The preparation method of the electrolyte specifically includes the following steps:
[0101] In a dry argon-atmospheric glove box, ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed in a mass ratio of EC:PC:EMC:DEC = 1:3:3:3. Then, fluoroethylene carbonate and 1,3-propane sulpholactone were added, dissolved, and thoroughly stirred. Lithium salt LiPF6 was then added and mixed evenly to obtain the electrolyte. The mass percentages of LiPF6, fluoroethylene carbonate, and 1,3-propane sulpholactone were all 12.5% and 2% respectively, calculated based on the mass of the electrolyte.
[0102] The preparation method of the separator membrane specifically includes the following steps:
[0103] Polyethylene porous polymer film is used as the separator.
[0104] The preparation method of lithium-ion batteries specifically includes the following steps:
[0105] The negative electrode sheet provided in this embodiment is cut into a circular piece with a diameter of 14 mm as the working electrode, and a lithium metal sheet with a diameter of 18 mm is used as the reference electrode. The two are separated by a separator with a diameter of 20 mm. An appropriate amount of electrolyte is added, and the CR2430 coin cell lithium-ion battery is assembled.
[0106] Performance testing methods:
[0107] First Coulomb Efficiency Test
[0108] The button cell battery was tested using a blue battery tester. The test procedure was as follows: Step 1: Discharge at 0.05C to 0V; Step 2: Rest for 5 minutes; Step 3: Discharge at 50μA to 0V; Step 4: Rest for 5 minutes; Step 5: Discharge at 20μA to 0V; Step 6: Rest for 5 minutes; Step 7: Charge at 0.1C to 2V; Step 8: Rest for 5 minutes. Steps 1 to 8 were repeated twice. Then, the battery was discharged at 1C to 0V, rested for 5 minutes, and charged at 0.1C to 2V, ending the test. The cumulative capacity of the first, third, and fifth discharge stages in the first cycle is the discharge capacity. Charging at 0.1C to 2.0V gives the charging capacity. Dividing the charging capacity by the weight of the modified graphite material gives the specific capacity of the modified graphite material. Dividing the charging capacity by the discharge capacity gives the initial coulombic efficiency.
[0109] Electrochemical impedance spectroscopy (EIS) testing
[0110] Electrochemical impedance spectroscopy (EIS) of coin-type lithium-ion batteries at 0°C was performed using a Solartron 1470E / 1455 electrochemical workstation (UK). The charge transfer resistance (Rct) was obtained through refined EIS analysis. Charging and discharging capacities were also measured at 0.05C.
[0111] The button cell battery was tested using a blue battery tester. The test procedure was as follows: Step 1: Discharge at 0.05C to 0V; Step 2: Rest for 5 minutes; Step 3: Discharge at 50μA to 0V; Step 4: Rest for 5 minutes; Step 5: Discharge at 20μA to 0V; Step 6: Rest for 5 minutes; Step 7: Charge at 0.1C to 2V; Step 8: Rest for 5 minutes. Steps 1 to 8 were repeated twice. Then, the battery was discharged at 1C to 0V, rested for 5 minutes, and then charged at 0.1C to 2V. The test was then completed. The cumulative capacity of the three discharge stages (steps 1, 3, and 5) is the discharge capacity. The charging capacity is obtained by charging at 0.1C to 2.0V.
[0112] 1C charging and discharging capacity test
[0113] The button cell battery was tested using a blue battery tester. The test procedure was as follows: First, discharge at 1C to 0V; second, let it stand for 5 minutes; third, charge at 0.1C to 2V. The test was then completed. The discharge capacity is obtained during the first discharge process, and the charging capacity is obtained by charging at 0.1C to 2.0V in the third step.
[0114] The modified graphite materials (or graphite materials), negative electrode sheets, or lithium-ion batteries of Examples 1-2 to 1-25 and Comparative Example 1 differ from Example 1 only in that the oxygen content, Id / Ig, and water contact angle of the negative electrode sheet at 25°C are adjusted according to Table 1. The graphite material of Comparative Example 1 is the untreated artificial graphite raw material of Example 1.
[0115] Table 1
[0116]
[0117]
[0118] As shown in Table 1, compared with the graphite material of Comparative Example 1, the modified graphite material of this application has carbonyl groups, which, when combined with the honeycomb structure on the substrate, can improve the first coulombic efficiency, charging capacity and discharging capacity of lithium-ion batteries. It can also reduce the charge transfer internal resistance and improve the charging capacity and discharging capacity at the rate, thus improving the energy density and kinetic performance of lithium-ion batteries.
[0119] In particular, this application, based on the presence of carbonyl groups in the modified graphite material, can further improve the lithium intercalation capacity and kinetic performance of the modified graphite material when the oxygen content is controlled within the above-mentioned range.
[0120] In particular, by controlling the Id / Ig value of the modified graphite material in this application and coordinating it with the aforementioned carbonyl groups, the lithium intercalation capacity and kinetic performance can be further improved.
[0121] In particular, the modified graphite material of this application can achieve a lower water contact angle when applied in the electrode, which is beneficial to improving the compatibility and wettability of the modified graphite material in the electrode with the electrolyte, reducing electrode polarization and charge transfer resistance, thereby further improving the dynamic performance of the electrode.
[0122] The scanning tunneling microscope (STM) characterization images of the basal surface of the modified graphite materials in Examples 1-22 are shown below. Figure 1 As shown, the base surface exhibits a partially collapsed and deformed honeycomb structure, which is understandable. Figure 1 The reason why the collapsed and deformed part does not show a honeycomb structure is that the voltage applied during the STM test to achieve sufficient resolution is too large, which causes the interaction force between the tip and the sample to damage the sample structure.
[0123] Figure 2 The infrared spectra of the modified graphite materials of Examples 1-22 and the graphite material of Comparative Example 1 are shown, wherein the graphite material of Comparative Example 1 is the untreated artificial graphite raw material of Example 1. In the infrared spectra of the modified graphite materials of Examples 1-22, at 1560 cm⁻¹... -1 The presence of a characteristic peak of carbonyl (-C=O) that can adsorb lithium ions indicates that the modified graphite materials of Examples 1-22 have carbonyl groups, while the graphite material of Comparative Example 1 does not have this characteristic peak.
[0124] Figure 3 Electrochemical impedance spectroscopy (EIS) spectra of the modified graphite materials of Examples 1-22 and the graphite material of Comparative Example 1 are shown. The EIS spectra show that the charge transfer resistance (Rct) of the modified graphite material provided in this application is reduced by about 10 mΩ, and it has higher kinetics.
[0125] Figure 4The table shows the charging and discharging capacity test data of coin-type lithium-ion batteries prepared with the modified graphite materials of Examples 1-22 and the graphite material of Comparative Example 1 under 0.05C discharge / 0.1C charging conditions. Combined with the data in Table 1, it can be seen that compared with the graphite material of Comparative Example 1, the modified graphite material provided in this application increases the 0.05C charging capacity by approximately 7 mAh / g and the 1C discharging capacity by approximately 31 mAh / g. Therefore, the graphite material of this application can improve the negative electrode capacity and kinetics, resulting in a lithium-ion battery with high energy density and fast charging performance.
[0126] The above description is merely a preferred embodiment of this application and is not intended to limit this application. Any modifications, equivalent substitutions, and improvements made within the principles of this application should be included within the protection scope of this application.
Claims
1. A modified graphite material, characterized in that, The modified graphite material has a honeycomb structure on its basal surface, and its infrared spectrum contains a characteristic peak of carbonyl groups, located at 1550 cm⁻¹. -1 Up to 1570cm -1 between; The oxygen content on the surface of the modified graphite material is O, with a mass content of 0.5% ≤ O ≤ 1.8%. In the Raman spectrum of the modified graphite material, the value of Id / Ig ranges from 0.1194 to 0.1505.
2. The modified graphite material according to claim 1, characterized in that, 1.2% ≤ 0 ≤ 1.8%; and / or, 0.132≤Id / Ig≤0.1505.
3. The modified graphite material according to claim 1 or 2, characterized in that, The modified graphite material satisfies at least one of conditions 1 to 5: Condition 1: The average particle size d of the modified graphite material is 11.2 μm ≤ d ≤ 24.7 μm; Condition 2: The specific surface area (BET) of the modified graphite material is 0.8 m². 2 / g≤BET≤2.2 m 2 / g; Condition 3: The specific capacity (cpg) of the modified graphite material is 341 mAh / g ≤ cpg ≤ 364 mAh / g; Condition 4: The compacted density (cd) of the modified graphite material under 5000 kg pressure is 1.72 g / cm³. 3 ≤cd≤2.08 g / cm 3 ; Condition 5: The degree of graphitization (gd) of the modified graphite material is 91% ≤ gd ≤ 97%.
4. The method for preparing the modified graphite material according to any one of claims 1 to 3, characterized in that, Includes the following steps: providing graphite; The modified graphite material is obtained by heat treatment of the graphite in an ozone-containing atmosphere. The temperature te for the heat preservation treatment is 50℃≤te≤200℃, and the time ti is 1 h≤ti≤10 h. The volume concentration vc of ozone in the ozone-containing atmosphere is 2% ≤ vc ≤ 10%.
5. The preparation method according to claim 4, characterized in that, The graphite is selected from synthetic graphite and / or natural graphite; and / or, 110℃≤te≤150℃, 2 h≤ti≤5 h; and / or, 5% ≤ vc ≤ 8%; and / or, The volumetric flow rate (vfr) of the ozone-containing atmosphere is 500 mL / min ≤ vfr ≤ 3000 mL / min.
6. A negative electrode sheet, characterized in that, The modified graphite material includes any one of claims 1 to 3 or the modified graphite material prepared by the preparation method described in claim 4 or 5.
7. The negative electrode sheet according to claim 6, characterized in that, The water contact angle θ of the negative electrode at 25°C is 82°≤θ≤110°.
8. The negative electrode sheet according to claim 6, characterized in that, The water contact angle θ of the negative electrode at 25°C is 82°≤θ≤88°.
9. A secondary battery, characterized in that, The secondary battery includes the negative electrode sheet as described in any one of claims 6 to 8.
10. An electronic device, characterized in that, The electronic device includes the secondary battery as described in claim 9.
Citation Information
Patent Citations
Preparation process of silane coupling agent composite modified graphite lithium ion battery negative electrode material
CN117577798A