Blast furnace slag solid waste-based concrete and preparation process thereof

By combining cement, ferric chloride, and carboxylic acid compounds containing sulfonic acid groups, the problem of low compressive strength in blast furnace slag concrete was solved, and the compressive strength of blast furnace slag solid waste-based concrete was improved.

CN118439834BActive Publication Date: 2026-11-24LANGFANG HENGDE NEW MATERIALS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410709902.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-03
Publication Date
2026-11-24
Estimated Expiration
2044-06-03

AI Technical Summary

Technical Problem

Concrete prepared from blast furnace slag using existing technologies has relatively low compressive strength.

Method used

By using a specific ratio of cement, ferric chloride, and carboxylic acid compounds containing sulfonic acid groups, calcium chloride is generated through the hydration reaction of ferric chloride and cement, which increases the density of concrete. At the same time, the sulfonic acid groups promote cement hydration to generate more calcium chloride, thereby improving compressive strength.

Benefits of technology

It significantly improved the compressive strength of blast furnace slag solid waste-based concrete.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of concrete technology, and proposes a blast furnace slag solid waste-based concrete and its preparation process. The blast furnace slag solid waste-based concrete comprises the following components in parts by weight: 25-30 parts cement, 185-195 parts blast furnace slag, 5-10 parts silica fume, 3-8 parts fly ash, 0.5-1 part bentonite powder, 0.4-1 part water-reducing agent, 15-20 parts water, 0.5-2.5 parts ferric chloride, and 0.1-1.7 parts carboxylic acid compounds containing sulfonic acid groups. This technical solution solves the problem of low compressive strength in concrete prepared from blast furnace slag in existing technologies.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of concrete technology, specifically to a blast furnace slag solid waste-based concrete and its preparation process. Background Technology

[0002] Blast furnace slag is a solid waste generated during the ironmaking process. Based on different chemical compositions, blast furnace slag can be classified into alkaline blast furnace slag, acidic blast furnace slag, high-alumina blast furnace slag, high-titanium blast furnace slag, fluorine-containing blast furnace slag, and ferromanganese blast furnace slag, etc. It can be used as an admixture for cement and concrete and is a good "secondary resource".

[0003] Applying blast furnace slag to concrete can not only effectively utilize industrial waste and reduce costs, but also improve the concrete's impermeability, durability, and corrosion resistance. However, its compressive strength needs further improvement. Summary of the Invention

[0004] This invention proposes a blast furnace slag solid waste-based concrete and its preparation process, which solves the problem of low compressive strength of blast furnace slag-based concrete in related technologies.

[0005] The technical solution of the present invention is as follows: A blast furnace slag solid waste-based concrete comprises the following components in parts by weight: 25-30 parts cement, 185-195 parts blast furnace slag, 5-10 parts silica fume, 3-8 parts fly ash, 0.5-1 parts bentonite powder, 0.4-1 parts water-reducing agent, 15-20 parts water, 0.5-2.5 parts ferric chloride, and 0.1-1.7 parts carboxylic acid compounds containing sulfonic acid groups.

[0006] As a further technical solution, the mass ratio of cement to ferric chloride is 28:1~2.

[0007] This invention limits the mass ratio of cement to ferric chloride to 28:1~2, which further improves the compressive strength of blast furnace slag solid waste-based concrete.

[0008] As a further technical solution, the mass of the ferric chloride is greater than the mass of the carboxylic acid compound containing a sulfonic acid group.

[0009] As a further technical solution, the mass of the ferric chloride is ≥ 2 times the mass of the carboxylic acid compound containing sulfonic acid groups.

[0010] As a further technical solution, the mass ratio of the ferric chloride to the carboxylic acid compound containing sulfonic acid groups is 1.4: 0.3~0.5.

[0011] This invention limits the mass ratio of ferric chloride to carboxylic acid compounds containing sulfonic acid groups to 1.4:0.3~0.5, which further improves the compressive strength of blast furnace slag solid waste-based concrete.

[0012] As a further technical solution, the carboxylic acid compound containing a sulfonic acid group includes one or two of sulfoacetic acid and 6-sulfononaphthalene-1,4-dicarboxylic acid.

[0013] As a further technical solution, the cement is ordinary Portland cement PO 32.5.

[0014] As a further technical solution, the blast furnace slag contains 38.65 wt% CaO, 0.8 wt% Fe2O3, 27.35 wt% SiO2, 7.36 wt% MgO, 0.02 wt% P2O5, 13.19 wt% Al2O3, 0.54 wt% MnO, 8.47 wt% TiO2, and 1.87 wt% SO3.

[0015] As a further technical solution, the water-reducing agent includes one or two of naphthalene-based water-reducing agents and polycarboxylate water-reducing agents.

[0016] The present invention also proposes a preparation process for blast furnace slag solid waste-based concrete, comprising the following steps: mixing the components in the specified mass fractions evenly to obtain blast furnace slag solid waste-based concrete.

[0017] The working principle and beneficial effects of this invention are as follows: The addition of ferric chloride and carboxylic acid compounds containing sulfonic acid groups in this invention synergistically improves the compressive strength of concrete prepared from blast furnace slag. Ferric chloride reacts with calcium hydroxide precipitated during cement hydration, generating calcium chloride that fills the concrete, improving its density. Simultaneously, the carboxyl and sulfonic acid groups in the carboxylic acid compounds promote cement hydration, generating even more calcium chloride that fills the concrete, thereby increasing the compressive strength of the blast furnace slag-based concrete. Detailed Implementation

[0018] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0019] The parameters of the raw materials in the following examples and comparative examples are as follows: The cement is ordinary Portland cement PO 32.5; The blast furnace slag contains 38.65 wt% CaO, 0.8 wt% Fe2O3, 27.35 wt% SiO2, 7.36 wt% MgO, 0.02 wt% P2O5, 13.19 wt% Al2O3, 0.54 wt% MnO, 8.47 wt% TiO2, and 1.87 wt% SO3. It is composed of particles with a mass ratio of 3:20:35:32:6:4, with particle sizes >4.75 mm, 4.75 mm ≥ >2.36 mm, 2.36 mm ≥ >1.18 mm, 1.18 mm ≥ >0.6 mm, 0.6 mm ≥ >0.3 mm, and 0.3 mm ≥ >0.16 mm. It originates from Chengde Iron and Steel Group. The silicon content in the silicon micro powder is ≥95wt%, and the particle size is 200 mesh; The fly ash is Grade I fly ash with a particle size of 600 mesh; The bentonite powder has an expansion ratio of 15, a montmorillonite content of ≥95wt%, an apparent viscosity of 15mPa·s, and a particle size of 3000 mesh. The polycarboxylate superplasticizer is Sika superplasticizer 530P; The naphthalene-based water-reducing agent is Point-N200, a high-efficiency naphthalene-based water-reducing agent.

[0020] Example 1 Mix 28 parts cement, 190 parts blast furnace slag, 8 parts silica fume, 5 parts fly ash, 0.8 parts bentonite powder, 0.5 parts ferric chloride, and 1.7 parts sulfoacetic acid for 5 minutes. Then, while stirring, add 0.7 parts polycarboxylate superplasticizer and 18 parts water and continue mixing for 2 minutes to obtain blast furnace slag solid waste-based concrete.

[0021] Example 2 Mix 25 parts cement, 185 parts blast furnace slag, 5 parts silica fume, 3 parts fly ash, 0.5 parts bentonite powder, 0.5 parts ferric chloride, and 1.7 parts 6-sulfononaphthalene-1,4-dicarboxylic acid for 5 minutes. Then, while stirring, add 0.4 parts polycarboxylate superplasticizer and 20 parts water and continue mixing for 2 minutes to obtain blast furnace slag solid waste-based concrete.

[0022] Example 3 Mix 30 parts cement, 195 parts blast furnace slag, 10 parts silica powder, 8 parts fly ash, 1 part bentonite powder, 0.5 parts ferric chloride, and 1.7 parts sulfoacetic acid for 5 minutes. While stirring, add 1 part naphthalene-based water-reducing agent and 15 parts water and continue mixing for 2 minutes to obtain blast furnace slag solid waste-based concrete.

[0023] Example 4 Mix 28 parts cement, 190 parts blast furnace slag, 8 parts silica fume, 5 parts fly ash, 0.8 parts bentonite powder, 1 part ferric chloride, and 1.7 parts sulfoacetic acid for 5 minutes. While stirring, add 0.7 parts polycarboxylate superplasticizer and 18 parts water and continue mixing for 2 minutes to obtain blast furnace slag solid waste-based concrete.

[0024] Example 5 Mix 28 parts cement, 190 parts blast furnace slag, 8 parts silica fume, 5 parts fly ash, 0.8 parts bentonite powder, 1.4 parts ferric chloride, and 1.7 parts sulfoacetic acid for 5 minutes. While stirring, add 0.7 parts polycarboxylate superplasticizer and 18 parts water and continue mixing for 2 minutes to obtain blast furnace slag solid waste-based concrete.

[0025] Example 6 Mix 28 parts cement, 190 parts blast furnace slag, 8 parts silica fume, 5 parts fly ash, 0.8 parts bentonite powder, 2 parts ferric chloride, and 1.7 parts sulfoacetic acid for 5 minutes. Then, while stirring, add 0.7 parts polycarboxylate superplasticizer and 18 parts water and continue mixing for 2 minutes to obtain blast furnace slag solid waste-based concrete.

[0026] Example 7 Mix 28 parts cement, 190 parts blast furnace slag, 8 parts silica fume, 5 parts fly ash, 0.8 parts bentonite powder, 2.5 parts ferric chloride, and 1.7 parts sulfoacetic acid for 5 minutes. While stirring, add 0.7 parts polycarboxylate superplasticizer and 18 parts water and continue mixing for 2 minutes to obtain blast furnace slag solid waste-based concrete.

[0027] Example 8 Mix 28 parts cement, 190 parts blast furnace slag, 8 parts silica fume, 5 parts fly ash, 0.8 parts bentonite powder, 1.4 parts ferric chloride, and 1.2 parts sulfoacetic acid for 5 minutes. Then, while stirring, add 0.7 parts polycarboxylate superplasticizer and 18 parts water and continue mixing for 2 minutes to obtain blast furnace slag solid waste-based concrete.

[0028] Example 9 Mix 28 parts cement, 190 parts blast furnace slag, 8 parts silica fume, 5 parts fly ash, 0.8 parts bentonite powder, 1.4 parts ferric chloride, and 0.7 parts sulfoacetic acid for 5 minutes. Then, while stirring, add 0.7 parts polycarboxylate superplasticizer and 18 parts water and continue mixing for 2 minutes to obtain blast furnace slag solid waste-based concrete.

[0029] Example 10 Mix 28 parts cement, 190 parts blast furnace slag, 8 parts silica fume, 5 parts fly ash, 0.8 parts bentonite powder, 1.4 parts ferric chloride, and 0.5 parts sulfoacetic acid for 5 minutes. Then, while stirring, add 0.7 parts polycarboxylate superplasticizer and 18 parts water and continue mixing for 2 minutes to obtain blast furnace slag solid waste-based concrete.

[0030] Example 11 Mix 28 parts cement, 190 parts blast furnace slag, 8 parts silica fume, 5 parts fly ash, 0.8 parts bentonite powder, 1.4 parts ferric chloride, and 0.3 parts sulfoacetic acid for 5 minutes. Then, while stirring, add 0.7 parts polycarboxylate superplasticizer and 18 parts water and continue mixing for 2 minutes to obtain blast furnace slag solid waste-based concrete.

[0031] Example 12 Mix 28 parts cement, 190 parts blast furnace slag, 8 parts silica fume, 5 parts fly ash, 0.8 parts bentonite powder, 1.4 parts ferric chloride, and 0.1 parts sulfoacetic acid for 5 minutes. Then, while stirring, add 0.7 parts polycarboxylate superplasticizer and 18 parts water and continue mixing for 2 minutes to obtain blast furnace slag solid waste-based concrete.

[0032] Comparative Example 1 Mix 28 parts cement, 190 parts blast furnace slag, 8 parts silica fume, 5 parts fly ash, 0.8 parts bentonite powder, and 2.2 parts ferric chloride for 5 minutes. While mixing, add 0.7 parts polycarboxylate superplasticizer and 18 parts water and continue mixing for 2 minutes to obtain blast furnace slag solid waste-based concrete.

[0033] Comparative Example 2 Mix 28 parts cement, 190 parts blast furnace slag, 8 parts silica fume, 5 parts fly ash, 0.8 parts bentonite powder, and 2.2 parts sulfoacetic acid for 5 minutes. While stirring, add 0.7 parts polycarboxylate superplasticizer and 18 parts water and continue mixing for 2 minutes to obtain blast furnace slag solid waste-based concrete.

[0034] Comparative Example 3 Mix 28 parts cement, 190 parts blast furnace slag, 8 parts silica fume, 5 parts fly ash, and 0.8 parts bentonite powder for 5 minutes. While mixing, add 0.7 parts polycarboxylate superplasticizer and 18 parts water and continue mixing for 2 minutes to obtain blast furnace slag solid waste-based concrete.

[0035] The blast furnace slag solid waste-based concrete obtained in Examples 1-12 and Comparative Examples 1-3 were cured in a standard curing room in accordance with GB / T 50081-2019, and then prepared into standard specimens. The compressive strength was tested at 7 days and 28 days, and the test results are recorded in Table 1.

[0036] Table 1 Compressive strength of blast furnace slag solid waste-based concrete

[0037] As can be seen from Table 1, the blast furnace slag solid waste-based concrete provided by the present invention has high compressive strength.

[0038] Compared with Comparative Examples 1-3, Examples 1-12 added ferric chloride and carboxylic acid compounds containing sulfonic acid groups, Comparative Example 1 added ferric chloride, Comparative Example 2 added carboxylic acid compounds containing sulfonic acid groups, and Comparative Example 3 did not add ferric chloride and carboxylic acid compounds containing sulfonic acid groups. The compressive strength of the blast furnace slag solid waste-based concrete obtained in Examples 1-12 was higher than that in Comparative Examples 1-3, indicating that the combined use of ferric chloride and carboxylic acid compounds containing sulfonic acid groups synergistically improved the compressive strength of the blast furnace slag solid waste-based concrete.

[0039] The compressive strength of the blast furnace slag solid waste-based concrete obtained in Examples 4-6 is higher than that in Examples 1 and 7, indicating that the mass ratio of cement to ferric chloride of 28:1-2 can further improve the compressive strength of the blast furnace slag solid waste-based concrete.

[0040] The compressive strength of the blast furnace slag solid waste-based concrete obtained in Examples 10-11 is higher than that of the other examples, indicating that the mass ratio of ferric chloride to carboxylic acid compounds containing sulfonic acid groups is 1.4:0.3-0.5, which can further improve the compressive strength of the blast furnace slag solid waste-based concrete.

[0041] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A type of blast furnace slag solid waste-based concrete, characterized in that, The composition comprises the following components in parts by weight: 25-30 parts cement, 185-195 parts blast furnace slag, 5-10 parts silica fume, 3-8 parts fly ash, 0.5-1 part bentonite powder, 0.4-1 part water-reducing agent, 15-20 parts water, 0.5-2.5 parts ferric chloride, and 0.1-1.7 parts of a carboxylic acid compound containing a sulfonic acid group, wherein the carboxylic acid compound containing a sulfonic acid group includes one or two of sulfoacetic acid and 6-sulfononaphthalene-1,4-dicarboxylic acid; the mass ratio of cement to ferric chloride is 28:1-2; and the mass of ferric chloride is ≥2 times the mass of the carboxylic acid compound containing a sulfonic acid group.

2. The blast furnace slag solid waste-based concrete according to claim 1, characterized in that, The mass ratio of ferric chloride to a carboxylic acid compound containing a sulfonic acid group is 1.4:0.3~0.

5.

3. The blast furnace slag solid waste-based concrete according to claim 1, characterized in that, The cement is ordinary Portland cement PO 32.

5.

4. The blast furnace slag solid waste-based concrete according to claim 1, characterized in that, The blast furnace slag contains 38.65 wt% CaO, 0.8 wt% Fe2O3, 27.35 wt% SiO2, 7.36 wt% MgO, 0.02 wt% P2O5, 13.19 wt% Al2O3, 0.54 wt% MnO, 8.47 wt% TiO2, and 1.87 wt% SO3.

5. The blast furnace slag solid waste-based concrete according to claim 1, characterized in that, The water-reducing agent includes one or two of naphthalene-based water-reducing agents and polycarboxylate water-reducing agents.

6. The preparation process of blast furnace slag solid waste-based concrete according to any one of claims 1 to 5, characterized in that, Includes the following steps: The components of the specified mass fraction are mixed evenly to obtain blast furnace slag solid waste-based concrete.

Citation Information

Patent Citations

  • Micro-powder co-doped full-industrial solid waste concrete and preparation method thereof

    CN111635194A