A multi-oxide cavitation-resistant coating and a method for preparing the same
By preparing a single-layer multi-element oxide coating on the surface of the flow-through components of a hydro-generator set, the equipment problems caused by cavitation erosion were solved, achieving a high-hardness and thermally stable anti-cavitation effect, and extending the service life of the components.
Patent Information
- Application Number
- CN202410343992.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-25
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-03-25
AI Technical Summary
In the existing technology, the flow-through components of hydro turbine generator sets face problems such as increased equipment vibration, noise and severe corrosion and wear under cavitation. Moreover, the existing coatings are insufficient in terms of thermal stability and hardness, and cannot effectively extend the service life of the components.
A single-layer multi-element oxide coating containing metal elements such as Al, Cr, Ti, Zr, V, Fe, Ni, and Co is deposited on the surface of the flow-through component by reactive magnetron sputtering. The coating has a single-phase polycrystalline face-centered cubic crystal structure, with oxygen atoms connected to metal atoms by ionic bonds. The oxygen content to metal element ratio is 0.85–1.25:1, and the coating thickness is 1.5–7.5 μm. The coating is prepared using a mixture of argon and oxygen gas.
The coating has high hardness, good adhesion and wear resistance, which can extend the service life of components in cavitation-resistant environments and maintain structural stability at high temperatures, thus improving the service performance of hydro-generator units.
Smart Images

Figure CN118441243B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of surface engineering technology, specifically relating to an anti-cavitation multi-element oxide coating and its preparation method. Background Technology
[0002] Large hydro-turbine generator units operate under prolonged conditions of water flow impact, severely impacted by cavitation. Cavitation refers to the formation of bubbles or cavities in flowing liquids. This phenomenon typically occurs at high liquid velocities or low pressures, where gas in the liquid is stripped out to form bubbles, leading to localized pressure drops. Cavitation not only reduces the effective flow area of the liquid and decreases fluid transfer efficiency but can also cause increased vibration, noise, and accelerated corrosion and wear on equipment surfaces. The intensity of cavitation in hydro-turbines is primarily influenced by material and environmental factors. Material factors include the material's microstructure, mechanical properties, and surface finish, while environmental factors include water flow conditions, water temperature, and second-phase characteristics. Modifying and strengthening the material surface can effectively improve the turbine's resistance to cavitation without replacing the entire material of the flow-through components. Coating technology, a type of surface strengthening technology, improves the surface strength of materials by applying a thin film or coating. Coating preparation processes are simple, offer excellent performance, and are low-cost, playing a significant role in the cavitation resistance of flow-through components.
[0003] The protective coating on the surface of flow-through components not only requires good mechanical properties, wear resistance, and oxidation resistance, but also excellent adhesion to prevent it from being detached by water flow during use. Magnetron sputtering is a commonly used surface coating technology that transforms materials from a solid state to a gaseous state and then deposits them as a thin film on the surface of the target object. The coatings prepared by this method have excellent adhesion, density, and uniformity, which can meet the requirements for the preparation of protective coatings on the surface of relevant components of hydro-generator sets.
[0004] In the selection of coating materials, high-entropy materials with multiple principal components have attracted widespread attention due to their excellent comprehensive mechanical properties. As a ceramic material, oxides have a lower formation energy than nitrides and carbides, thus exhibiting better thermodynamic stability. Furthermore, since oxide coatings do not react with oxygen, they will not fail due to reactions in the service environment. This invention provides a high-entropy oxide coating containing multiple principal components for cavitation resistance of flow-through components in hydro-generator sets. Summary of the Invention
[0005] The purpose of this section is to outline some aspects of embodiments of the present invention and to briefly describe some preferred embodiments. Simplifications or omissions may be made in this section, as well as in the abstract and title of this application, to avoid obscuring the purpose of these documents; however, such simplifications or omissions should not be construed as limiting the scope of the invention.
[0006] In view of the problems existing in the above and / or prior art, the present invention is proposed.
[0007] Therefore, the purpose of this invention is to overcome the shortcomings of the prior art and provide a cavitation-resistant multi-element oxide coating.
[0008] To solve the above-mentioned technical problems, the present invention provides the following technical solution: the coating is a single-layer oxide coating, comprising,
[0009] (i) It is composed of oxygen atoms and metal atoms;
[0010] (ii) is a single-phase polycrystalline face-centered cubic crystal structure;
[0011] (iii) Oxygen atoms are connected to metal atoms by ionic bonds;
[0012] (iv) The ratio of oxygen content to total metallic element content is 0.85 to 1.25:1;
[0013] (v) The content of each metal element is the same.
[0014] As a preferred embodiment of the anti-cavitation multi-element oxide coating of the present invention, the metal elements include 4 to 6 of Al, Cr, Ti, Zr, V, Fe, Ni and Co.
[0015] As a preferred embodiment of the anti-cavitation erosion multi-element oxide coating of the present invention, the coating has the following characteristics:
[0016] (i) The overall thickness of the coating is 1.5–7.5 μm;
[0017] (ii) Hardness is 20-35 GPa;
[0018] (iii) The membrane-substrate bonding strength is 20–35 N.
[0019] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for preparing an anti-cavitation multi-element oxide coating.
[0020] To solve the above-mentioned technical problems, the present invention provides the following technical solution: the coating is prepared by reactive magnetron sputtering, comprising,
[0021] After the surface of the flow-through component to be coated is pretreated, it is installed into the cavity of the magnetron sputtering coating machine, and the target is mounted on the target gun of the equipment. The vacuum degree in the cavity is controlled to be <1×10. -6 Torr;
[0022] Argon and oxygen are simultaneously introduced into the cavity, and the vacuum level of the cavity is controlled to be 0.5–1.5 × 10⁻⁶. -2 Torr;
[0023] Rotate the base station and apply a DC bias voltage of 65-225V to the base;
[0024] Radio frequency voltage is applied to the target gun, and an anti-cavitation multi-element oxide coating is deposited on the surface of the current-carrying component for a deposition time of 45–350 min.
[0025] As a preferred embodiment of the method for preparing the anti-cavitation multi-element oxide coating according to the present invention, the pretreatment includes polishing or cleaning; wherein the cleaning is performed using acetone and alcohol to remove impurities and oil film from the surface of the component.
[0026] In a preferred embodiment of the method for preparing anti-cavitation multi-element oxide coatings according to the present invention, the flow-through component is installed in the cavity of the magnetron sputtering coating instrument by fixing the flow-through component on a rotatable substrate fixing stage, and the surface to be coated is exposed on the side facing the target material.
[0027] In a preferred embodiment of the method for preparing the anti-cavitation multi-element oxide coating of the present invention, the rotation speed of the substrate fixing stage is 5 to 35 rpm.
[0028] As a preferred embodiment of the method for preparing the anti-cavitation erosion multi-element oxide coating of the present invention, the target material includes 2 to 4 of the following eight pure metal targets: Al, Cr, Ti, Zr, V, Fe, Ni, and Co, or four alloy targets: AlCr, TiZr, VNi, and FeCo.
[0029] In a preferred embodiment of the method for preparing the anti-cavitation multi-element oxide coating of the present invention, the flow rate of argon gas is 20-35 sccm, and the ratio of the flow rate of oxygen gas to the flow rate of argon gas is 1:2 to 2:1.
[0030] In a preferred embodiment of the method for preparing the anti-cavitation erosion multi-element oxide coating of the present invention, the target gun is subjected to a radio frequency voltage with a power density of 5.25–8.25 W / cm². 2 The radio frequency is 115-130MHz.
[0031] Beneficial effects of this invention:
[0032] (1) The multi-element oxide coating prepared by the present invention has advantages such as high hardness, good wear resistance, thermal stability and mechanical properties. Moreover, it does not react with oxygen in the environment during long-term service, so it can obtain a longer service life in cavitation-resistant environments.
[0033] (2) The present invention uses a simple preparation process to obtain a cavitation erosion resistant coating with good performance, which can effectively extend the service life of flow components. Attached Figure Description
[0034] To more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings used in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort. Wherein:
[0035] Figure 1 The X-ray diffraction pattern is shown for the multi-component oxide coating obtained in Example 1 of this invention.
[0036] Figure 2 This is a scanning electron microscope image of the surface of the multi-element oxide coating obtained in Example 1 of the present invention.
[0037] Figure 3 This is a scanning electron microscope (SEM) image of the interface of the multi-component oxide coating obtained in Example 1 of the present invention. Detailed Implementation
[0038] To make the above-mentioned objects, features and advantages of the present invention more apparent and understandable, the specific embodiments of the present invention will be described in detail below with reference to the examples in the specification.
[0039] Many specific details are set forth in the following description in order to provide a full understanding of the invention. However, the invention may also be practiced in other ways different from those described herein, and those skilled in the art can make similar extensions without departing from the spirit of the invention. Therefore, the invention is not limited to the specific embodiments disclosed below.
[0040] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The phrase "in one embodiment" appearing in different places in this specification does not necessarily refer to the same embodiment, nor is it a single or selective embodiment that is mutually exclusive with other embodiments.
[0041] Unless otherwise specified, all raw materials used in this invention are commercially available.
[0042] The materials obtained in the embodiments of the present invention were subjected to performance testing according to the following method:
[0043] The crystal structure was tested using an X-ray diffractometer (Bruker, D8 Advance Davinci).
[0044] Composition and morphology were determined using a scanning electron microscope (FEI, Quanta 250FEG) equipped with an energy dispersive spectrometer.
[0045] The hardness of the coating was tested using a nanoindenter (MTS, NANO G200);
[0046] The adhesion test was conducted using an automatic scratch tester (Zhongke Kaihua, WS-2005). Specifically, a scratch was made on the coating surface until a small crack appeared at the edge of the scratch. The normal pressure of the scratch is the adhesion force between the coating and the film substrate.
[0047] The wear resistance of the coating was tested using an Anton Paar (HVTRB) friction and wear tester. A 6mm diameter stainless steel ball was used as the grinding pair, the normal pressure was set to 10N, the friction reciprocating length was 5mm, the frequency was 2Hz, and the test time was 60min.
[0048] The thermal stability of the coating was tested using a high-temperature tube furnace at a temperature of 1000℃ for 5 hours in an air environment.
[0049] Example 1
[0050] This embodiment provides a method for preparing a multi-element oxide coating, specifically as follows:
[0051] Using 304 stainless steel sheet and amorphous quartz sheet as the substrate, the surface of the substrate is polished with 4000 grit sandpaper to remove the oxide layer and contaminants on the surface of the substrate.
[0052] Clean the polished substrate surface with acetone and alcohol, and then thoroughly dry the substrate surface with nitrogen.
[0053] Mount the substrate sheet onto the substrate mounting stage in the cavity of the magnetron sputtering coating machine, ensuring that the side to be coated faces the target gun.
[0054] FeCo, AlCr, and pure Ni metal targets were mounted on a target gun. The elemental content of the FeNi and AlCr targets was 1:1. The FeCo and Ni targets were mounted on a strong magnetic target gun. The targets were disc-shaped, with a diameter of 10.16 cm and a thickness of 1.5 mm. The effective deposition area of the targets was 81 cm². 2 ;
[0055] Close the chamber door of the coating apparatus and use a mechanical pump and a molecular pump to evacuate the vacuum level in the chamber to 0.5 × 10⁻⁶. - 6 Torr;
[0056] Argon and oxygen are slowly introduced into the cavity simultaneously. The argon flow rate is 25 sccm, and the oxygen flow rate ratio to the argon flow rate is 3:5. The vacuum level of the cavity is controlled to be 0.9 × 10⁻⁶ by adjusting the opening and closing of the valve between the vacuum pump and the cavity. - 2 Torr;
[0057] The base station is rotated at 15 rpm, and a DC bias of 155V is applied to the base.
[0058] A 560W RF voltage was applied to a target gun containing FeCo, a 460W RF voltage was applied to a target gun containing AlCr, both with an RF frequency of 115MHz, and a 510W RF voltage was applied to a target gun containing Ni with an RF frequency of 125MHz.
[0059] By opening the baffle between the substrate and the target gun, a coating is prepared on the substrate. The opening time of the baffle is controlled to ensure that the deposition time is 270 minutes, thus obtaining a multi-element oxide coating.
[0060] Figure 1 The figure shows the X-ray diffraction pattern of the multi-component oxide coating obtained in Example 1 of this invention. As can be seen from the figure, the X-ray diffraction peaks only appeared at 39.7°, 44.9°, 68.8° and 82.6°. The positions of these four diffraction peaks are completely consistent with those of face-centered cubic crystals, indicating that the coating is a single-phase face-centered cubic (FCC) crystal structure and does not contain other phases.
[0061] Figure 2 The image shows a scanning electron microscope (SEM) image of the multi-element oxide coating obtained in Example 1 of this invention. As can be seen from the image, the coating has a polycrystalline structure and the grain size is uniform at ~125 nm, indicating that the coating of this invention is a single-phase polycrystalline crystal.
[0062] Figure 3 The image shows a scanning electron microscope (SEM) image of the interface of the multi-element oxide coating obtained in Example 1 of this invention. As can be seen from the image, the coating is grown in columnar crystal form, is dense and has no obvious structural defects, and has a thickness of ~2 μm.
[0063] Example 2
[0064] The difference between this embodiment and Example 1 is that the FeCo target material is changed to a VNi target material, while the element content ratio of the VNi target material remains 1:1. The rest of the preparation process is the same as in Example 1, and a multi-element oxide coating is obtained.
[0065] Example 3
[0066] The difference between this embodiment and Example 1 is that the FeCo target material is changed to a TiZr target material, while the element content ratio of the TiZr target material remains 1:1. The rest of the preparation process is the same as in Example 1, and a multi-element oxide coating is obtained.
[0067] The performance of the materials prepared in the above embodiments was tested, and the results compared with those of Example 1 are shown in Table 1.
[0068] Table 1
[0069] Example 1 Example 2 Example 3 Crystal structure FCC FCC FCC Thickness (μm) 2 1.2 1.1 Hardness (GPa) 34.7 25.9 24.3 Binding force (N) 35 28.5 26.6 <![CDATA[Wear rate (mm 3 / Nm)]]> <![CDATA[3.6×10 -6 ]]> <![CDATA[1.7×10 -4 ]]> <![CDATA[1.9×10 -4 ]]> Crystal structure after 5 hours of oxidation FCC FCC+Body-Centered Cube (BCC) FCC+Body-Centered Cube (BCC)
[0070] As can be seen from the table above, adjusting the target material has a significant impact on the performance of the multi-element oxide coating. This is because the types and contents of elements in the coating significantly affect the ratio of ionic bonds to metallic bonds. Only when the ratio reaches a certain equilibrium can the optimal coating performance be obtained. According to the results in the table above, the best technical effects can be obtained when FeCo, AlCr, and pure Ni metal targets are selected in this invention.
[0071] Example 4
[0072] The difference between this embodiment and Example 1 is that the ratio of oxygen flow rate to argon content is adjusted to 0.5:1, while the rest of the preparation process is the same as in Example 1, resulting in a multi-element oxide coating.
[0073] Example 5
[0074] The difference between this embodiment and Example 1 is that the ratio of oxygen flow rate to argon content is adjusted to 1:1, while the rest of the preparation process is the same as in Example 1, to obtain a multi-element oxide coating.
[0075] Example 6
[0076] The difference between this embodiment and Example 1 is that the ratio of oxygen flow rate to argon content is adjusted to 2:1, while the rest of the preparation process is the same as in Example 1, to obtain a multi-element oxide coating.
[0077] The performance of the materials prepared in the above embodiments was tested, and the results compared with those of Example 1 are shown in Table 2.
[0078] Table 2
[0079] Example 1 Example 4 Example 5 Example 6 Crystal structure FCC FCC FCC FCC Thickness (μm) 2 2.6 2.8 2.9 Hardness (GPa) 34.7 23.7 22.4 20.1 Binding force (N) 35 20.9 22.3 21.4 <![CDATA[Wear rate (mm 3 / Nm)]]> <![CDATA[3.6×10 -6 ]]> <![CDATA[7.5×10 -5 ]]> <![CDATA[5.8×10 -5 ]]> <![CDATA[5.1×10 -5 ]]> Crystal structure after 5 hours of oxidation FCC FCC+BCC FCC+BCC FCC+BCC
[0080] As shown in the table above, adjusting the oxygen content has a significant impact on the performance of the multi-component oxide coating. This is because the ratio of oxygen to argon directly affects the degree of reaction between sputtered metal atoms and oxygen atoms, thereby altering the content and types of oxides in the coating. Increasing the oxygen flow rate increases the oxidation degree, potentially leading to the formation of more oxide phases or even different oxides. This not only affects the overall composition and crystal structure of the coating but also causes a decrease in coating hardness due to excessive oxidation. An appropriate oxygen content can improve the chemical bonding between the coating and the substrate, enhancing the adhesion. Based on the results in the table above, the optimal technical effect is achieved when the oxygen to nitrogen flow rate ratio in this invention is 3:5.
[0081] Comparative Example 1
[0082] This comparative example provides a method for preparing a conventional TiN coating, specifically as follows:
[0083] Using 304 stainless steel sheet and amorphous quartz sheet as the substrate, the surface of the substrate is polished with 4000 grit sandpaper to remove the oxide layer and contaminants on the surface of the substrate.
[0084] Clean the polished substrate surface with acetone and alcohol, and then thoroughly dry the substrate surface with nitrogen.
[0085] Mount the substrate sheet onto the substrate mounting stage in the cavity of the magnetron sputtering coating machine, ensuring that the side to be coated faces the target gun.
[0086] A pure Ti metal target was mounted on the target gun. The target was in the shape of a disc, 10.16 cm in diameter and 1.5 mm thick, with an effective deposition area of 81 cm². 2 ;
[0087] Close the chamber door of the coating apparatus, and use a mechanical pump and a molecular pump to evacuate the vacuum level in the chamber to 1×10⁻⁶. -6 Torr;
[0088] Argon and nitrogen gases are slowly introduced into the cavity simultaneously, with an argon flow rate of 16 sccm and a nitrogen flow rate of 10 sccm. The vacuum level of the cavity is controlled to be 0.5 × 10⁻⁶ by adjusting the opening and closing of the valve between the vacuum pump and the cavity. -2 Torr;
[0089] The base station is rotated at a speed of 20 rpm, and a DC bias of 50V is applied to the base.
[0090] A 250W DC voltage was applied to the target gun containing Ti, and the baffle between the substrate and the target gun was opened. A coating was prepared on the substrate, and the opening time of the baffle was controlled to ensure that the deposition time was 150min.
[0091] Comparative Example 2
[0092] This comparative example provides a method for preparing an existing Al2O3 coating, specifically as follows:
[0093] Using 304 stainless steel sheet and amorphous quartz sheet as the substrate, the surface of the substrate is polished with 4000 grit sandpaper to remove the oxide layer and contaminants on the surface of the substrate.
[0094] Clean the polished substrate surface with acetone and alcohol, and then thoroughly dry the substrate surface with nitrogen.
[0095] Mount the substrate sheet onto the substrate mounting stage in the cavity of the magnetron sputtering coating machine, ensuring that the side to be coated faces the target gun.
[0096] An Al2O3 ceramic target was mounted on the target gun. The target was in the shape of a disc, with a diameter of 10.16 cm and a thickness of 1.5 mm. The effective deposition area of the target was 81 cm². 2 ;
[0097] Close the chamber door of the coating apparatus and use a mechanical pump and a molecular pump to evacuate the vacuum level in the chamber to 0.2 × 10⁻⁶. - 6 Torr;
[0098] Argon gas is slowly introduced into the cavity at a flow rate of 16 sccm. The vacuum level of the cavity is controlled to be 1×10⁻⁶ by adjusting the opening and closing of the valve between the vacuum pump and the cavity. -2 Torr;
[0099] Rotate the base station at a speed of 20 rpm;
[0100] A 300W radio frequency voltage was applied to the Al2O3 target gun, the radio frequency frequency was 100MHz, the baffle between the substrate and the target gun was opened, and a coating was prepared on the substrate. The opening time of the baffle was controlled to ensure that the deposition time was 300min.
[0101] The performance of the materials prepared in the above comparative example was tested, and the results compared with those of Example 1 are shown in Table 3.
[0102] Table 3
[0103] Example 1 Comparative Example 1 Comparative Example 2 Crystal structure FCC TiN <![CDATA[Al2O3]]> Thickness (μm) 2 4.48 0.72 Hardness (GPa) 34.7 16.7 39.7 Bonding force (N) 35 26.9 18.6 <![CDATA[Wear rate (mm 3 / Nm)]]> <![CDATA[3.6×10 -6 ]]> <![CDATA[2.3×10 -4 ]]> <![CDATA[5.4×10 -5 ]]> Crystal structure after 5 hours of oxidation FCC <![CDATA[TiO2+TiN]]> <![CDATA[Al2O3]]>
[0104] As shown in the table above, the hardness of the multi-element oxide coating prepared by this invention can reach 34.7 GPa; the adhesion between the coating and the 304 stainless steel substrate is 35 N; and the wear rate of the coating is 3.6 × 10⁻⁶. -6 mm 3 / Nm; The coating was placed in a tube furnace for oxidation at 1000℃, and the structural changes of the coating were tested again. The coating remained FCC crystals, indicating that the coating has good thermal stability. Although the two existing coatings are superior to the multi-element oxide coating provided by this invention in some aspects, they cannot meet the requirements of the cavitation resistance of the coating for the flow components of the hydro-generator set due to defects such as insufficient thermal stability, poor hardness, and insufficient thickness.
[0105] In summary, this invention discloses an anti-cavitation multi-element oxide coating and its preparation method. This coating can be applied to the surface of flow-through components of large hydro-generator sets to improve the components' resistance to water flow cavitation. The coating provided by this invention contains 4 to 6 metallic elements, with each element having a substantially equal content. The oxygen content to the total metallic element content is 0.85 to 1.25:1, and the oxygen atoms in the coating are interconnected with the metal atoms by ionic bonds. The coating is a single layer with a total thickness of 1.5 to 7.5 μm. The coating is prepared using reactive magnetron sputtering technology, with a mixture of oxygen and argon gas introduced into the wall as the reactive gas, and co-sputtering using 2 to 4 alloy targets. The oxide coating provided by this invention exhibits excellent adhesion, high hardness, and excellent mechanical properties, possessing good wear resistance and anti-cavitation performance, and is expected to significantly extend the service life of flow-through components in large hydro-generator sets.
[0106] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A cavitation erosion resistant multi-component oxide coating, characterized in that: The coating is a single-layer oxide coating, comprising: (i) Composed of oxygen atoms and metal atoms; (ii) is a single-phase polycrystalline face-centered cubic crystal structure; (iii) Oxygen atoms are connected to metal atoms by ionic bonds; (iv) The ratio of oxygen content to total metal content is 0.85~1.25∶1; (v) The content of each metallic element is the same; The metallic elements include 4 to 6 of the following: Al, Cr, Ti, Zr, V, Fe, Ni, and Co. The coating has the following characteristics: (i) The overall thickness of the coating is 1.5~7.5 μm; (ii) Hardness is 20~35 GPa; (iii) The membrane-substrate bonding strength is 20~35 N; The cavitation erosion resistant multi-component oxide coating is prepared by reactive magnetron sputtering, comprising, After the surface of the flow-through component to be coated is pretreated, it is installed into the cavity of the magnetron sputtering coating machine, and the target is mounted on the target gun of the equipment. The vacuum degree in the cavity is controlled to be <1×10. -6 Torr; Argon and oxygen are simultaneously introduced into the cavity, and the vacuum level of the cavity is controlled to be 0.5~1.5×10⁻⁶. -2 Torr; Rotate the base station and apply a DC bias voltage of 65~225 V to the base; Radio frequency voltage is applied to the target gun, and an anti-cavitation multi-element oxide coating is deposited on the surface of the current-flowing component for a deposition time of 45~350 min.
2. The method for preparing the cavitation erosion resistant multi-component oxide coating as described in claim 1, characterized in that: The pretreatment includes polishing or cleaning; wherein the cleaning is performed using acetone and alcohol to remove impurities and oil film from the surface of the component.
3. The method for preparing the cavitation erosion resistant multi-component oxide coating as described in claim 1, characterized in that: The flow-through component is installed in the cavity of the magnetron sputtering coating instrument to fix the flow-through component on a rotatable substrate fixing stage, with the surface to be coated exposed on the side facing the target.
4. The method for preparing the cavitation erosion resistant multi-component oxide coating as described in claim 1, characterized in that: The rotation speed of the base fixing stage is 5~35 rpm.
5. The method for preparing the cavitation erosion resistant multi-component oxide coating as described in claim 1, characterized in that: The target material includes eight pure metal targets (Al, Cr, Ti, Zr, V, Fe, Ni, Co) or two to four alloy targets (AlCr, TiZr, VNi, FeCo).
6. The method for preparing the cavitation erosion resistant multi-component oxide coating as described in claim 1, characterized in that: The flow rate of the argon gas is 20-35 sccm, and the ratio of the flow rate of the oxygen gas to the flow rate of the argon gas is 1:2 to 2:
1.