Method for calculating the fatigue life of axial-radial cracks in the inner wall of longitudinal welds of cylinders

By measuring the yield strength and stress intensity factor, and combining cyclic alternating loads and the medium environment, a crack propagation rate model was established, which solved the problem of inaccurate calculation of the fatigue propagation life of axial and radial cracks in the inner wall of the longitudinal weld of a cylinder, and realized a simple and efficient engineering application.

CN118443495BActive Publication Date: 2026-11-20HEFEI GENERAL MACHINERY RES INST
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410419699.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-09
Publication Date
2026-11-20
Estimated Expiration
2044-04-09

AI Technical Summary

Technical Problem

Existing technologies fail to effectively consider the effects of welding residual stress and service environment when calculating the fatigue propagation life of axial and radial cracks on the inner wall of longitudinal weld seams of cylinders. This results in inaccurate calculation results and a complex calculation process, making it difficult to apply to engineering practice.

Method used

A method is adopted to establish a crack propagation rate model by measuring the yield strength and stress intensity factor, combined with cyclic alternating load and medium environment, and to calculate the crack propagation life, taking into account the influence of welding residual stress and medium environment.

Benefits of technology

A simple and efficient calculation method is provided, which can accurately predict crack propagation life. It is applicable to the design and operation stages and improves the engineering practicality of the calculation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118443495B_ABST
    Figure CN118443495B_ABST
Patent Text Reader

Abstract

The present application belongs to the technical field of high-pressure container design and failure assessment, and particularly relates to a method for calculating the fatigue expansion life of axial and radial cracks in the inner wall of a longitudinal weld of a cylinder. The present application comprises the following steps: determining the structural parameters of a high-pressure thick-walled welded cylinder and a cyclic alternating load condition, and obtaining the shape parameters of an initial crack in the inner wall of a longitudinal weld and a heat-affected zone of the cylinder; calculating the stress intensity factor of the deepest point and the free surface of the initial crack under the cyclic alternating load condition; measuring the fracture toughness or stress corrosion fracture toughness of the test piece, building a crack expansion rate calculation model of the test piece under the driving action of the cyclic alternating load and the service medium environment, and performing crack expansion calculation to obtain the fatigue expansion life. The present application simultaneously considers the influence of the cylinder under the bearing of internal and external pressure loads, welding residual stress and service medium environment, has the advantages of efficient and simple calculation process and high accuracy of calculation results, and has high practicability in engineering calculation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of high-pressure vessel design, development and failure assessment, specifically relating to a method for calculating the fatigue propagation life of axial-radial cracks on the inner wall of a cylindrical longitudinal weld. Background Technology

[0002] In engineering applications, most high-pressure vessels adopt a plate-welded structure, which is formed by rolling and welding thick-walled plates. Welding is a metallurgical process with uneven heating (large temperature difference). The internal microstructure of the weld and heat-affected zone has coarse grains. Coupled with the influence of workpiece restraint, the workpiece will undergo yielding deformation during the welding process, resulting in large residual stresses in the weld and heat-affected zone after cooling. Welding residual stress is very destructive because during the service of high-pressure vessels, welding residual stress will continuously superimpose the primary and secondary stresses generated during the vessel's load-bearing process, resulting in a large superimposed stress. This is also the reason why most welded vessels are prone to cracking in the weld and heat-affected zone. Engineering practice shows that compared with the pressure vessel base material, the weld and heat-affected zone are more prone to surface crack initiation, which then propagates rapidly under corrosive environments or fatigue conditions, leading to vessel rupture and failure.

[0003] According to plate and shell theory, the circumferential stress of a cylinder is twice that of the axial stress and is the first principal stress. Therefore, longitudinal welds and heat-affected zones are more prone to the initiation of axial-radial cracks, making fatigue propagation studies and safety assessments of these areas more significant in engineering. Since axial-radial cracks on the inner wall can usually be considered semi-elliptical, the calculation of the propagation of longitudinal welds containing axial-radial cracks on cylinders under corrosive environments or fatigue conditions, based on fracture mechanics theory, mainly involves the following steps: ① Calculate the stress intensity factor at the deepest point of the initial crack and at the free surface under cyclic alternating load conditions; ② Establish a crack propagation rate calculation model under cyclic alternating loads and service medium conditions; ③ Based on the initial crack, perform iterative calculations until the crack extends to the critical crack depth.

[0004] For crack fatigue propagation life, researchers currently rely primarily on the finite element method (FEM). However, due to the highly complex welding heating and cooling process involved in the longitudinal weld of a cylindrical vessel, the FEM struggles to accurately simulate the input loads and boundary conditions during welding, leading to significant discrepancies between simulated residual stresses and actual values. Furthermore, calculating crack fatigue propagation life using the FEM requires modeling, loading, calculating, and solving the cracked structure, resulting in a substantial workload, and the accuracy is significantly affected by the finite element mesh. Therefore, the FEM numerical method is not suitable for calculating the fatigue propagation life of weld cracks in engineering applications. Additionally, while ASME BPVC.Ⅷ.3-2023 "Another Construction Code for High Pressure Vessels" and GB / T34019—2017 "Ultra-High Pressure Vessels" mention typical cracks in high-pressure vessels, they explicitly state that they are not applicable to welded structures because these standards do not consider the influence of residual welding stresses. Therefore, when calculating the fatigue propagation life of cracks initiating in the weld and heat-affected zone of high-pressure plate welded vessels, engineers often do not consider the influence of welding residual stress.

[0005] As can be seen from the existing situation, the calculation of crack fatigue propagation life for cylindrical containers, which are welded components, is inherently prone to inaccuracies due to the rigid finite element method and the neglect of residual welding stress. Therefore, in practical engineering applications, finding a simpler, more efficient, and more comprehensive method for calculating the crack fatigue propagation life of axial-radial cracks in the inner wall of longitudinal welds in cylindrical containers is particularly important. Summary of the Invention

[0006] The purpose of this invention is to overcome the shortcomings of the prior art and provide a method for calculating the axial-radial crack fatigue propagation life of the inner wall of a cylindrical longitudinal weld. This invention simultaneously considers the influence of internal and external pressure loads, welding residual stress, and the service environment on the vessel. Therefore, it is specifically applicable to the calculation process of crack fatigue propagation life of the inner wall of a cylindrical longitudinal weld during the design and operation stages. It also has the advantages of efficient and concise calculation process and high accuracy of calculation results, making it highly practical in engineering calculations.

[0007] To achieve the above objectives, the present invention adopts the following technical solution: A method for calculating the fatigue propagation life of axial-radial cracks on the inner wall of a longitudinal weld seam in a cylinder, characterized by the following steps: S1. Determine the structural parameters and cyclic alternating load conditions of the high-pressure thick-walled welded cylinder, and obtain the shape parameters of the initial cracks on the inner wall of the longitudinal weld seam and heat-affected zone of the cylinder; S2. Calculate the stress intensity factor at the deepest point of the initial crack and at the free surface under cyclic alternating load conditions, specifically including: S2.1. Prepare a test specimen of the longitudinal welded joint of the cylinder and measure the yield strength of the specimen at the working temperature; S2.2. Calculate the baseline fitting coefficients under the initial and final operating conditions. A i ',in, i It is an integer, and 0 ≤ i ≤3: ①If the cylinder has not undergone post-weld heat treatment, then:

[0008] in, p i The pressure load inside the cylinder is expressed in MPa. K It is the ratio of the outer diameter to the inner diameter of the cylinder; p o The external pressure load on the cylinder is expressed in MPa. R t p0.2 The measured yield strength of the specimen at the operating temperature is expressed in MPa. ②If the cylinder undergoes heat treatment after welding, then:

[0009] Subsequently, obtained by calculation A i ′, fit the stress distribution in the plane perpendicular to the axial radial crack of the inner wall under the initial and final working conditions; S2.3. Calculate the actual fitting coefficients under the initial and final operating conditions using the following formula. A i :

[0010] In the formula, a The depth of the semi-elliptical crack, in units mm ; t For the wall thickness of the cylinder, in units mm ; Then, the shape factor of the axial-radial crack in the inner wall was calculated. Q The stress intensity factors at the deepest point of the initial radial crack in the inner wall and at the free surface under the initial and final working conditions are obtained. S3. Measure the fracture toughness or stress corrosion fracture toughness of the specimen, establish a crack propagation rate calculation model of the specimen under cyclic alternating load and service medium environment, and perform crack propagation calculation to obtain fatigue propagation life.

[0011] Preferably, in step S2.2, the stress distribution perpendicular to the plane of the axial-radial crack in the inner wall under the initial and final working conditions is... The fitting formula is:

[0012] In the formula, x The distance measured from the free surface of the crack is denoted by , where is the variable and is in units of . mm And 0≤ x ≤ t .

[0013] Preferably, in step S2.3, the shape factor of the axial-radial crack on the inner wall... Q The calculation formula is:

[0014] In the formula, l The length of the semi-elliptical crack, in units. mm.

[0015] Preferably, in step S2.3, the stress intensity factor at the deepest point of the initial radial crack in the inner wall and at the free surface under the initial and final working conditions is... K I for:

[0016] In the formula, G 0、 G 1. G 2 and G 3 are all stress intensity factor influence coefficients, which are dimensionless.

[0017] Preferably, in step S1, the structural parameters of the high-pressure thick-walled welded cylinder include: the outer radius of the cylinder, the inner radius of the cylinder, the base material and welding material used in the cylinder, and the cylinder welding process; the cyclic alternating load conditions include the pressure load and temperature load under the initial and final conditions of the cylinder; the shape parameters of the initial cracks in the inner wall of the longitudinal weld seam and heat-affected zone of the cylinder include the semi-elliptical crack depth and the semi-elliptical crack length, which are determined by non-destructive testing methods.

[0018] Preferably, in step S3, the fracture toughness or stress corrosion fracture toughness of the specimen is obtained by testing a three-point bending specimen or a CT specimen; the specimen is subjected to a pre-crack fatigue propagation test in the service medium environment by means of a three-point bending specimen or a CT specimen to obtain a crack propagation rate calculation model.

[0019] Preferably, in step S3, when performing crack propagation calculations, the critical crack depth is determined based on the fracture toughness of the specimen. K IC or stress corrosion fracture toughness K ISCC The critical value was used, and the trend of the semi-elliptical crack depth and length as the number of cycles increased was obtained through crack propagation calculation. Then, the step size Δ was gradually reduced. a The total number of cycles required to propagate the crack to the critical crack depth was obtained using this method. N p and the total number of cycles extending to 0.25 times the critical crack depth N c ,Pick N p / 2 and N c The smaller of these values ​​represents the fatigue extended life.

[0020] Preferably, after obtaining the fatigue extension life, the semi-elliptical crack depth and semi-elliptical crack length corresponding to the fatigue extension life are the final allowable crack depth and crack length; during the service of the high-pressure thick-walled welded cylinder, when the monitored actual crack depth and actual crack length do not exceed the final allowable crack depth and crack length, the actual crack is safe; otherwise, a risk alarm is triggered.

[0021] The beneficial effects of this invention are as follows: 1) The calculation method proposed in this invention not only considers the stress caused by pressure load, but also the residual stress generated during the welding heating and cooling process and the service medium environment, which are important influencing factors. It has high feasibility and the calculation results are more accurate. It also provides engineers with a quantitative analysis method for the fatigue propagation life and safety evaluation of such cracks, and solves the current technical problems.

[0022] 2) The calculation method proposed in this invention does not require the use of finite element calculation software, and has a complete calculation process applicable to the crack fatigue propagation life of the inner wall of the longitudinal weld of a cylinder during the design and operation stages. The calculation is highly targeted and the calculation process is fast and simple, making it highly practical in engineering calculations. Attached Figure Description

[0023] Figure 1 This is a flowchart of the calculation process of the present invention; Figure 2 This is a stress distribution trend diagram perpendicular to the plane where the crack is located, caused by internal and external pressure loads and welding thermal deformation, as shown in Example 1. Figure 3 This is a comparison chart of the fitting curve and the original stress distribution data using the present invention in Example 1; Figure 4 This is a graph showing the variation trend of stress intensity factor at the deepest point and the free surface during crack propagation in Example 1. Figure 5 The image shows the trend of the depth and length of the semi-elliptical crack during the crack propagation process in Example 1, as well as the final allowable crack depth and crack length. Figure 6 This is a diagram showing the safety and risk range of a semi-elliptical crack during crack propagation in Example 1. Detailed Implementation

[0024] For ease of understanding, this section combines... Figures 1-6 The calculation method proposed in this invention is further described below: For high-pressure, thick-walled welded cylinders subjected to pressure loads on both their inner and outer walls, the morphology and stress structure of axial-radial cracks initiating in the longitudinal weld and heat-affected zone are crucial. Under alternating fatigue loads, these cracks will gradually grow until the vessel becomes unstable and ruptures. The calculation of fatigue propagation life in the longitudinal weld and heat-affected zone of the cracked cylinder is primarily based on the theory of linear elastic fracture mechanics and consists of the following process: ① Calculate the stress intensity factor at the deepest point and the free surface of the initial crack in the longitudinal weld and heat-affected zone of the cylinder under cyclic alternating load conditions; ②Establish a calculation model for crack propagation rate under cyclic alternating loads and service environment conditions; ③ Based on the initial crack, perform iterative calculations until the crack depth is reached.

[0025] Meanwhile, for a high-pressure thick-walled welded cylinder (hereinafter referred to as the cylinder) whose inner and outer walls are subjected to pressure loads, the stress perpendicular to the plane of the axial-radial crack on the inner wall of the cylinder can be mathematically derived as follows:

[0026] In the formula, The stress is perpendicular to the plane of the axial-radial crack on the inner wall of the cylinder. It is caused by internal and external pressure loads and belongs to the category of primary stress. The unit is MPa. p i The pressure load inside the cylinder is expressed in MPa. p o The external pressure load on the cylinder is expressed in MPa. r i The inner radius of the cylinder, in units mm ; r o The outer radius of the cylinder, in units mm ; K It is the ratio of the outer diameter to the inner diameter of the cylinder;x The distance measured from the free surface of the crack, in units of... mm .

[0027] At this point, the residual welding stress in the longitudinal weld seam and heat-affected zone of the cylinder can be categorized into two cases: ① If the cylinder has not undergone post-weld heat treatment, the residual welding stress perpendicular to the plane of the axial-radial crack on the inner wall of the cylinder can be calculated using the following formula:

[0028] In the formula, The residual stress in the plane of the axial-radial crack in the inner wall of the cylinder (in the longitudinal weld and heat-affected zone) is caused by thermal deformation during the welding process and belongs to the category of secondary stress. The unit is MPa. R t p0.2 The measured yield strength of the longitudinal welded joint specimen of the cylinder at the working temperature is expressed in MPa. t For the wall thickness of the cylinder, in units mm .

[0029] ② If the cylinder undergoes a post-weld heat treatment process, the residual welding stress in the plane of the radial crack perpendicular to the inner wall of the cylinder can be calculated using the following formula:

[0030] For axial-radial cracks initiating in the longitudinal weld seam and heat-affected zone of the cylinder, the effects of primary stress and secondary stress (residual stress) should be comprehensively considered. Internal axial-radial cracks are typically semi-elliptical cracks; the calculation method for their fatigue propagation life can be further referred to... Figure 1 As shown, it is calculated through the following steps: D1. Determine the structural parameters of the cylinder, including: the outer radius of the cylinder, the inner radius of the cylinder, the materials used for the cylinder (including the base material and welding materials), and the welding process of the cylinder.

[0031] D2. Determine the cyclic alternating load conditions of the cylinder, including: pressure load and temperature load under the initial and final conditions.

[0032] D3. Measure the shape parameters of the initial cracks on the inner wall of the longitudinal weld seam and heat-affected zone of the cylinder, including the depth and length of the cracks; the size of the initial cracks can be determined by non-destructive testing methods.

[0033] D4. Calculate the stress intensity factor at the deepest point of the initial crack and at the free surface under cyclic alternating loading conditions, as follows: D4.1. Prepare a test specimen of the longitudinal welded joint of the cylindrical column (hereinafter referred to as the specimen) and measure the yield strength of the specimen at the working temperature.

[0034] The test specimen here should meet the following conditions: the test specimen should be welded at the extension of the longitudinal weld of the cylinder and the cylinder at the same time; the base material (including heat treatment state) and welding material of the test specimen should be consistent with those of the product during manufacturing; the test specimen should be welded by the welder of the welding vessel using the same conditions, process and welding technology as the welding vessel; the test specimen should be heat treated using the same process as the high pressure vessel where the cylinder is located.

[0035] D4.2. Fit the stress distribution in the plane perpendicular to the inner wall axial radial crack under the initial and final working conditions respectively using the following formula:

[0036] For thick-walled welded cylinders, there are two cases: ①If the cylinder has not undergone post-weld heat treatment, then:

[0037] ②If the cylinder undergoes heat treatment after welding, then:

[0038] D4.3. Calculate the actual fitting coefficients under the initial and final operating conditions using the following formula. A i :

[0039] In the formula, a The depth of the semi-elliptical crack is typically calculated by repeatedly performing the initial crack iterations for each crack growth step. (Unit: ...) mm ; D4.4. Calculate the shape factor of the axial-radial crack in the inner wall using the following formula. Q :

[0040] In the formula, l The length of the semi-elliptical crack, in units. mm ; D4.5. Calculate the stress intensity factor at the deepest point of the initial axial-radial crack and the free surface of the inner wall under the initial and final working conditions, respectively, using the following formula. K I :

[0041] In the formula, G i is the stress intensity factor influence coefficient, which is dimensionless.

[0042] D5. Test the fracture toughness or stress corrosion fracture toughness of the specimen.

[0043] When the material used in the cylinder is compatible with the medium, only the fracture toughness at room temperature needs to be tested. K IC Otherwise, stress corrosion crack toughness under corrosive conditions should be tested. K ISCC Typically, fracture toughness or stress corrosion cracking toughness can be obtained through three-point bending specimen testing or CT specimen testing.

[0044] D6. Establish a calculation model for crack propagation rate under cyclic alternating loads and service environment conditions.

[0045] The calculation model for crack fatigue growth rate is related to the materials used in the cylinder (including the base metal and welding materials), the welding process, and the environmental conditions in which it is used. Especially in corrosive environments, the same material may experience significantly faster crack growth than in air. Typically, the calculation model for crack growth rate of a specimen is obtained through pre-existing crack fatigue growth tests on three-point bending or CT specimens under specific environmental conditions. Calculation models for crack growth rate of different material types can be found in publicly available materials, usually the classic Paris equation, which will not be elaborated upon here.

[0046] D7. Perform crack propagation calculations.

[0047] Crack propagation calculation is an iterative solution based on the stress intensity factor calculation steps and the crack propagation rate calculation model. This is a dynamic calculation process; each crack growth step (i.e., increasing the step size Δ) involves a cyclical iteration. a This information is used as the initial calculation condition for the next step, and the calculation continues until the critical crack depth is reached. The critical crack depth can be determined using the classical stress intensity factor criterion, which is based on the fracture toughness of the specimen. K IC or stress corrosion fracture toughness K ISCC This is the critical value.

[0048] D8. Obtain fatigue propagation life and the final allowable crack depth and crack length.

[0049] By calculating crack propagation, we can obtain the trend graphs of the semi-elliptical crack depth and length as the number of cycles increases during the propagation process. Subsequently, we can obtain the total number of cycles required for the corresponding crack to propagate to the critical crack depth. N p and the total number of cycles extending to 0.25 times the critical crack depth N c . N p and N c The calculation uses a stepwise decrease of Δ aThe method was repeatedly tested until... N p and N c Until there is no significant change, or the change only occurs within a set threshold range. N p / 2 and N c The smaller value is the fatigue propagation life, and the corresponding crack depth and crack length are the final allowable crack depth and crack length.

[0050] D9. Establish crack safety and risk ranges to provide a basis for regular monitoring.

[0051] During the service life of high-pressure vessels, cracks should be tracked in real time and monitored regularly. A crack can be considered safe only when both the actual crack depth and length do not exceed the allowable limits; otherwise, it is considered a risk and alarms or other appropriate measures should be taken.

[0052] To facilitate a further understanding of the present invention, based on the above-described solution, the present invention also provides the following practical embodiments: Example 1 Assume a high-pressure vessel has a single-layer plate welded structure, where: Inner radius of cylinder r i It is 500mm, and the outer radius of the cylinder is r o The diameter is 800mm; the plate material is Q345R thick-walled plate, and the welding material is E5015-N2 (J507RH) high-toughness low-hydrogen welding rod. No post-weld heat treatment was performed (usually referring to insufficient overall post-weld heat treatment); internal pressure load of the cylinder. p i The external pressure load on the cylinder is 60 MPa. p o The pressure is 10 MPa, the operating temperature is room temperature, and the working medium inside the cylinder is air. It circulates within a pressure range of 0–60 MPa. Non-destructive testing of the longitudinal weld seam and heat-affected zone of the cylinder revealed an axial-radial crack on the inner wall. a It is 1mm. l It is 3mm.

[0053] The calculation method proposed in this invention is used to calculate crack fatigue life. The specific implementation steps include: 1. Calculate the stress intensity factor at the deepest point of the initial crack and at the free surface under cyclic alternating load conditions: The initial operating conditions of the container are: internal pressure 0MPa + external pressure 10MPa + room temperature; The final operating conditions are: internal pressure 60MPa + external pressure 10MPa + normal temperature.

[0054] The detailed calculations are as follows: 1.1. Calculate the stress distribution perpendicular to the crack plane caused by internal and external pressure loads and welding thermal deformation under the initial and final working conditions, respectively. Figure 2 As shown. Figure 2 This indicates that welding residual stress has a significant impact on the overall stress distribution trend, especially the tensile stress caused near the inner and outer surfaces, which has a significant impact on crack formation.

[0055] 1.2. Prepare test specimens of longitudinal welded joints of cylindrical cylinders, and measure the yield strength of the specimens at the operating temperature. R t p0.2 It is 380 MPa.

[0056] 1.3. Calculate the required baseline fitting coefficients in the fitting formulas for the initial and final operating conditions respectively. A i ′: Calculations show that under the initial operating conditions... A 0′~ A The 3′ values ​​are: 434.6, −3503.3, 6690.4, −3286.6; for the final state conditions. A 0′~ A The 3′ values ​​are: 571.5, −3617.0, 6769.3, and −3311.7.

[0057] The fitting curve plotted based on the obtained benchmark fitting coefficients is as follows: Figure 3 As shown. Figure 3 This indicates that the fitted curves under the initial and final working conditions basically coincide with the trends of the original stress distribution data, and the coefficient of determination of the fitted curves is... R 2 The statistic for measuring goodness of fit is 0.9999, indicating that the fitting accuracy is very high and the characterization effect is very good.

[0058] 1.4. Calculate the actual fitting coefficients A i .

[0059] Calculations show that under the initial operating conditions... A 0~ A The values ​​for 3 are: 434.6, -11.68, 0.074, and -0.00012, respectively; under the final state conditions. A 0~ A The values ​​are 571.5, −12.06, 0.075, and −0.00012, respectively.

[0060] 1.5. Calculate the shape factor at the deepest point of the crack and the free surface. Q The values ​​are 1.2384 and 1.3407 respectively.

[0061] 1.6. Calculations show that the stress intensity factor at the deepest point of the crack and at the free surface under the initial working conditions is... K I 20.78 MPa·m 1 / 2 18.38 MPa·m 1 / 2 Stress intensity factor at the deepest point of the crack and at the free surface under final operating conditions. K I 33.52 MPa·m 1 / 2 28.81 MPa·m 1 / 2 .

[0062] 2. Test the fracture toughness of the specimen in ambient air environment. K IC 160 MPa·m 1 / 2 .

[0063] 3. Establish a calculation model for crack propagation rate under cyclic alternating loads and service environment conditions, including: An experiment was conducted in a normal temperature air environment to determine the crack propagation rate calculation model for the longitudinal welded joint specimen of Q345R cylindrical steel, based on the standard Paris equation as follows:

[0064] In the formula, d a / d N d represents the crack propagation rate in the depth direction, in meters per crack. l / d N The crack propagation rate is measured in meters per crack. C 3.92×10 −12 Unit m / time (MPa·m 1 / 2 ) −m ; m It is 3.15, dimensionless; C and m These are all characteristic coefficients; Δ K I This represents the stress intensity factor amplitude, in MPa·m. 1 / 2 .

[0065] 4. Perform crack propagation calculations.

[0066] The calculation process is iterative; each step of crack growth serves as the initial calculation condition for the next step, until the critical crack depth is reached. The critical crack depth is determined by... K Imax= K IC = 160 MPa·m 1 / 2 The corresponding crack depth. During crack propagation, the trends of stress intensity factors at the deepest point of the crack and at the free surface under the initial and final working conditions are as follows: Figure 4 As shown.

[0067] Figure 4 This indicates that the critical crack depth is 50.0 mm, at which point the stress intensity factor at the free surface of the crack reaches the critical value under the final operating condition.

[0068] 5. Obtain fatigue propagation life and the final allowable crack depth and crack length.

[0069] During crack propagation, the trends in the depth and length of the semi-elliptical crack are as follows: Figure 5 As shown. Figure 5 This indicates that the crack depth and crack length exhibit a trend of initially slow growth followed by a significant rapid increase. By gradually decreasing Δ... a The method was repeatedly tested, and finally the step size Δ was chosen. a When the crack depth is 0.005 mm, the total number of cycles required for the crack to propagate to the critical crack depth of 50.0 mm is... N p =171,978 cycles, the total number of cycles required to extend the crack to 0.25 times the critical crack depth of 12.5 mm. N c = 141901 times.

[0070] Pick N p / 2 and N c The smaller value, 85989 cycles, represents the fatigue propagation life. The corresponding crack depth and crack length are the final allowable crack depth and crack length, i.e. Figure 5 The intersections are 3.33mm and 7.60mm respectively.

[0071] 6. Establish safe and risk ranges for cracks to provide a basis for regular monitoring.

[0072] During the service life of high-pressure vessels, actual cracks should be monitored regularly. When the crack depth and length of the monitored actual crack do not exceed 3.33 mm and 7.60 mm respectively, it is considered a cracked vessel. Figure 6 If the crack is within the safe zone, it can be considered safe; otherwise, there is a risk.

[0073] The above embodiments demonstrate that the calculation method proposed in this invention is feasible for calculating the fatigue propagation life of axial-radial cracks initiating in the longitudinal weld seam and heat-affected zone of a high-pressure vessel cylinder. This provides engineers with a method and basis for calculating the fatigue propagation life of cracks in such locations, solving current technical problems. This invention considers not only the stress caused by internal and external pressure loads, but also the residual stress generated during welding and the influence of the service environment. Furthermore, the entire calculation process does not require the use of other finite element calculation software or professional mathematical analysis software, ensuring speed and simplicity, facilitating engineering applications, and yielding significant results.

[0074] Of course, those skilled in the art will recognize that the present invention is not limited to the details of the exemplary embodiments described above, but also includes the same or similar methods that can be implemented in other specific forms without departing from the spirit or essential characteristics of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description.

[0075] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.

[0076] All technical parts not described in detail in this invention are publicly known technologies.

Claims

1. A method for calculating the fatigue propagation life of axial-radial cracks on the inner wall of a longitudinal weld seam in a cylinder, characterized in that... Includes the following steps: S1. Determine the structural parameters and cyclic alternating load conditions of the high-pressure thick-walled welded cylinder, and obtain the shape parameters of the initial cracks on the inner wall of the longitudinal weld seam and heat-affected zone of the cylinder; S2. Calculate the stress intensity factor at the deepest point of the initial crack and at the free surface under cyclic alternating load conditions, specifically including: S2.

1. Prepare a test specimen of the longitudinal welded joint of the cylinder and measure the yield strength of the specimen at the working temperature; S2.

2. Depending on whether the cylindrical body has undergone heat treatment, select one of the following: the baseline fitting coefficients for the initial and final working conditions, including the influence of primary stress and secondary residual stress of the weld seam distinguishing between heat treatment states. A i ',in, i It is an integer, and 0 ≤ i ≤3: ①If the cylinder has not undergone post-weld heat treatment, then: in, p i The pressure load inside the cylinder is expressed in MPa. K It is the ratio of the outer diameter to the inner diameter of the cylinder; p o The external pressure load on the cylinder is expressed in MPa. R t p0.2 The measured yield strength of the specimen at the operating temperature is expressed in MPa. ②If the cylinder undergoes heat treatment after welding, then: Subsequently, obtained by calculation A i ′, fit the stress distribution in the plane perpendicular to the axial radial crack of the inner wall under the initial and final working conditions; S2.

3. Calculate the actual fitting coefficients under the initial and final operating conditions using the following formula. A i : In the formula, a The depth of the semi-elliptical crack, in units mm ; t For the wall thickness of the cylinder, in units mm ; Then, the shape factor of the axial-radial crack in the inner wall was calculated. Q The stress intensity factors at the deepest point of the initial radial crack in the inner wall and at the free surface under the initial and final working conditions are obtained. S3. Measure the fracture toughness or stress corrosion fracture toughness of the specimen, establish a crack propagation rate calculation model of the specimen under cyclic alternating load and service medium environment, and perform crack propagation calculation to obtain fatigue propagation life.

2. The method for calculating the fatigue propagation life of axial-radial cracks on the inner wall of a longitudinal weld seam of a cylinder according to claim 1, characterized in that: In step S2.2, the stress distribution in the plane perpendicular to the axial-radial crack of the inner wall under the initial and final working conditions is described.   The fitting formula is: In the formula, x The distance measured from the free surface of the crack is denoted by , where is the variable and is in units of . mm And 0≤ x ≤ t .

3. The method for calculating the fatigue propagation life of axial-radial cracks on the inner wall of a longitudinal weld seam of a cylinder according to claim 2, characterized in that: In step S2.3, the shape factor of the axial-radial crack on the inner wall Q The calculation formula is: In the formula, l The length of the semi-elliptical crack, in units. mm .

4. The method for calculating the fatigue propagation life of axial-radial cracks on the inner wall of a longitudinal weld seam of a cylinder according to claim 3, characterized in that: In step S2.3, the stress intensity factor at the deepest point of the initial radial crack in the inner wall and at the free surface under the initial and final working conditions is... K I for: In the formula, G 0、 G 1. G 2 and G 3 are all stress intensity factor influence coefficients, which are dimensionless.

5. A method for calculating the fatigue propagation life of axial-radial cracks on the inner wall of a longitudinal weld seam of a cylinder according to claim 1, 2, 3, or 4, characterized in that: In step S1, the structural parameters of the high-pressure thick-walled welded cylinder are determined as follows: outer radius of the cylinder, inner radius of the cylinder, base material and welding material of the cylinder, and welding process of the cylinder; cyclic alternating load conditions include pressure load and temperature load under the initial and final conditions of the cylinder; the shape parameters of the initial cracks in the inner wall of the longitudinal weld seam and heat-affected zone of the cylinder include the semi-elliptical crack depth and semi-elliptical crack length, which are determined by non-destructive testing methods.

6. A method for calculating the fatigue propagation life of axial-radial cracks on the inner wall of a longitudinal weld seam of a cylinder according to claim 1, 2, 3, or 4, characterized in that: In step S3, the fracture toughness or stress corrosion fracture toughness of the specimen is obtained by testing the three-point bending specimen or CT specimen; the specimen is subjected to a pre-crack fatigue propagation test in the service medium environment by means of the three-point bending specimen or CT specimen to obtain a crack propagation rate calculation model.

7. The method for calculating the fatigue propagation life of axial-radial cracks on the inner wall of a longitudinal weld seam of a cylinder according to claim 6, characterized in that: In step S3, when performing crack propagation calculations, the critical crack depth is determined based on the fracture toughness of the specimen. K IC or stress corrosion fracture toughness K ISCC The critical value was used, and the trend of the semi-elliptical crack depth and length as the number of cycles increased was obtained through crack propagation calculation. Then, the step size Δ was gradually reduced. a The total number of cycles required to propagate the crack to the critical crack depth was obtained using this method. N p and the total number of cycles extending to 0.25 times the critical crack depth N c ,Pick N p / 2 and N c The smaller of these values ​​represents the fatigue extended life.

8. The method for calculating the fatigue propagation life of axial-radial cracks on the inner wall of a longitudinal weld seam of a cylinder according to claim 7, characterized in that: After obtaining the fatigue extension life, the semi-elliptical crack depth and semi-elliptical crack length corresponding to the fatigue extension life are the final allowable crack depth and crack length. During the service of the high-pressure thick-walled welded cylinder, if the monitored actual crack depth and actual crack length do not exceed the final allowable crack depth and crack length, then the actual crack is safe; otherwise, a risk alarm is triggered.

Citation Information

Patent Citations

  • Method for calculating stress axial-radial crack stress intensity factor of outer wall of ultrahigh pressure vessel cylinder

    CN113176142A

  • Method for calculating fatigue life of crack-containing stress concentration part

    CN117473839A