Preparation method and application of magnetic fly ash / nano-silver composite material
By preparing magnetic fly ash/nano-silver composite materials, the high cost and complexity of treating textile dyeing wastewater in existing technologies have been solved, achieving efficient dye removal and antibacterial effects, as well as rapid material recovery and resource utilization of fly ash.
Patent Information
- Application Number
- CN202410705048.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-03
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-06-03
AI Technical Summary
Existing methods for treating wastewater from the textile printing and dyeing industry and households involve complex steps, high costs, and high energy consumption. They also struggle to achieve the dual effects of dye removal and antibacterial action, and the difficulty in separating materials can lead to secondary pollution.
A magnetic fly ash/silver nanocomposite material was prepared. Silver nanoparticles were loaded through acidification, magnetic modification and reduction reaction, and combined with an external magnetic field to achieve efficient recovery and recycling of the material.
It achieves efficient antibacterial and degradation effects on dye wastewater, the material is easy to recycle and reuse, reducing treatment costs and realizing the resource utilization of fly ash.
Smart Images

Figure CN118454631B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of nano-silver composite materials technology, and in particular to a method for preparing and applying a magnetic fly ash / nano-silver composite material. Background Technology
[0002] The textile dyeing and printing industry, as well as households and laboratories, frequently discharge large quantities of wastewater containing unused organic dyes and pathogenic microorganisms into natural water bodies, causing widespread environmental pollution. Therefore, given the harmful effects of this wastewater on aquatic species and human health, developing effective measures for wastewater treatment and microbial control is urgent. To this end, a series of methods have been adopted, identifying some conventional technologies that can be effectively used for wastewater treatment, including filtration, ion exchange, precipitation, and advanced oxidation processes. However, these technologies have certain drawbacks, particularly the complexity of the steps involved, the high cost of purification operations, and high energy consumption. In contrast, adsorption processes offer a simple, low-cost, and environmentally friendly clean technology. Recent studies have reported on the adsorption capacity of biomass materials such as biochar, coal, and activated carbon for the purification of dye wastewater, but none have achieved the dual effect of dye removal and antibacterial activity. Furthermore, separating the treated materials from the dye wastewater is very difficult and can potentially lead to secondary pollution. Summary of the Invention
[0003] The technical problem this invention aims to solve is to overcome the shortcomings of existing technologies and provide a method for preparing and applying magnetic fly ash / nano-silver composite materials. The preparation method of this invention is simple, uses abundant raw materials, and allows for easy control of process parameters. It also achieves high-quality utilization of fly ash and solves the pollution problem of wastewater containing bacteria and dyes. The magnetic fly ash / nano-silver composite material prepared by this invention exhibits significant antibacterial and dye-degrading effects, and can be conveniently and efficiently recovered and reused from the aquatic environment using an external magnetic field.
[0004] The technical solution adopted by this invention to solve its technical problem is:
[0005] A method for preparing a magnetic fly ash / nano silver composite material, specifically including the following steps:
[0006] Step S1: Place fly ash in hydrochloric acid solution and stir. Filter and wash until neutral, then dry to obtain acidified fly ash.
[0007] Step S2: Add the acidified fly ash obtained in step S1 to a mixed solution composed of ferric chloride solution and ferrous sulfate solution and stir. After the magnetic stirrer is heated to 70°C, add 1 mol / L sodium hydroxide solution to adjust the pH to 8-9. Then place the beaker in an ultrasonic cleaner for ultrasonic dispersion for 30 min. After that, let it stand for 1 h to age. Filter and wash the precipitate until it is neutral and then dry it to obtain magnetic fly ash.
[0008] Step S3: The magnetic fly ash obtained in step S2 is soaked in AgNO3 solution in the dark and stirred continuously at room temperature; then the reducing agent trisodium citrate dihydrate is added and stirred continuously to carry out the reduction reaction to obtain nano-silver; finally, the magnetic fly ash containing nano-silver particles is filtered, dried and placed in a tube furnace and calcined at a heating rate of 10℃ / min under an inert atmosphere. After naturally cooling to room temperature, it is ground to obtain magnetic fly ash / nano-silver composite material.
[0009] Furthermore, in step S1, the mass percentage of hydrochloric acid solution is 5-20%, the solid-liquid ratio of fly ash to hydrochloric acid solution is 1:4 (g / mL), the stirring temperature is 90℃, and the stirring time is 1h.
[0010] Further, in step S2, the ferric chloride solution and ferrous sulfate solution are mixed in a volume ratio of 1:1, wherein the concentration of the ferric chloride solution is 0.12 mol / L and the concentration of the ferrous sulfate solution is 0.05 mol / L.
[0011] Furthermore, in step S2, the solid-liquid ratio of the acidified fly ash to the mixed solution is 1:20 (g / mL).
[0012] Furthermore, in step S3, the concentration of the AgNO3 solution is 0.05–0.9 g / L, and the solid-liquid ratio of the magnetic fly ash to the AgNO3 solution is 1:20 (g / mL).
[0013] Furthermore, in step S3, the ratio of the mass of trisodium citrate dihydrate to the concentration of AgNO3 solution is 1:2.5, and the reduction reaction time is 24 hours.
[0014] Furthermore, in step S3, the calcination temperature is 150–400°C, and the calcination time is 0.5–5 h.
[0015] An application of a magnetic fly ash / nano silver composite material, wherein the magnetic fly ash / nano silver composite material is prepared by the above preparation method, and the magnetic fly ash / nano silver composite material is used to inhibit bacteria and / or degrade dyes in bacterial dye wastewater.
[0016] The beneficial effects of this invention are as follows: This invention is rationally designed and has the following advantages:
[0017] (1) A highly active magnetic fly ash / nano silver composite material was prepared by loading nano silver onto a magnetically modified fly ash carrier. It has the dual function of killing common harmful bacteria in the environment (Escherichia coli, Staphylococcus aureus, Pseudomonas aeruginosa and Bacillus subtilis) and degrading azo dyes (methylene blue).
[0018] (2) The magnetic fly ash / nano silver composite material prepared by the present invention can be easily separated from the water environment by an external magnetic field, so as to realize the rapid recycling and reuse of the material.
[0019] (3) In addition, fly ash is a waste product of coal-fired power plants. Modifying it for dye degradation and antibacterial purposes is an economic and efficient way to realize the resource utilization and high-value utilization of fly ash.
[0020] (4) The preparation method of the present invention is simple and the preparation conditions are not harsh, which can realize large-scale production. Attached Figure Description
[0021] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.
[0022] Figure 1 These are SEM images of fly ash, magnetic fly ash, and the magnetic fly ash / nano silver composite material prepared in Example 1.
[0023] Figure 2 These are FT-IR images of fly ash, magnetic fly ash, and the magnetic fly ash / nano-silver composite material prepared in Example 1;
[0024] Figure 3 These are XRD patterns of fly ash, magnetic fly ash, and the magnetic fly ash / nano-silver composite material prepared in Example 1.
[0025] Figure 4 This is a magnetic separation diagram of the magnetic fly ash / nano silver composite material prepared in Example 1. Detailed Implementation
[0026] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of this application. Unless otherwise specified, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this application pertains.
[0027] It should be noted that the terminology used herein is for the purpose of describing particular implementations only and is not intended to limit the exemplary implementations according to this application. As used herein, the singular form includes the plural form unless the context clearly indicates otherwise. Furthermore, it should be understood that when the terms "comprising" and / or "including" are used in this description, they indicate the presence of features, steps, operations, devices, components, and / or combinations thereof.
[0028] The technical solution of the present invention will be clearly and completely described below with reference to the embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0029] A method for preparing a magnetic fly ash / nano silver composite material, specifically including the following steps:
[0030] Step S1: Place fly ash in hydrochloric acid solution and stir. Filter and wash until neutral, then dry to obtain acidified fly ash.
[0031] Step S2: Add the acidified fly ash obtained in step S1 to a mixed solution composed of ferric chloride solution and ferrous sulfate solution and stir. After the magnetic stirrer is heated to 70°C, add 1 mol / L sodium hydroxide solution to adjust the pH to 8-9. Then place the beaker in an ultrasonic cleaner for ultrasonic dispersion for 30 min. After that, let it stand for 1 h to age. Filter and wash the precipitate until it is neutral and then dry it to obtain magnetic fly ash.
[0032] Step S3: The magnetic fly ash obtained in step S2 is soaked in AgNO3 solution in the dark and stirred continuously at room temperature; then the reducing agent trisodium citrate dihydrate is added and stirred continuously to carry out the reduction reaction to obtain nano-silver; finally, the magnetic fly ash containing nano-silver particles is filtered, dried and placed in a tube furnace and calcined at a heating rate of 10℃ / min under an inert atmosphere. After naturally cooling to room temperature, it is ground to obtain magnetic fly ash / nano-silver composite material.
[0033] In step S1, the hydrochloric acid solution has a mass percentage of 10%, the solid-liquid ratio of fly ash to hydrochloric acid solution is 1:4 (g / mL), the stirring temperature is 90℃, and the stirring time is 1h.
[0034] In step S2, ferric chloride solution and ferrous sulfate solution are mixed in a volume ratio of 1:1, wherein the concentration of ferric chloride solution is 0.12 mol / L and the concentration of ferrous sulfate solution is 0.05 mol / L; the solid-liquid ratio of acidified fly ash to mixed solution in step S2 is 1:20 (g / mL).
[0035] In step S3, the concentration of the AgNO3 solution is 0.05–0.9 g / L, and the solid-liquid ratio of magnetic fly ash to AgNO3 solution is 1:20 (g / mL). In step S3, the mass ratio of trisodium citrate dihydrate to AgNO3 solution concentration is 1:2.5, and the reduction reaction time is 24 h. In step S3, the calcination temperature is 150–400℃, and the calcination time is 0.5–5 h.
[0036] An application of the magnetic fly ash / nano silver composite material prepared by the above preparation method, wherein the magnetic fly ash / nano silver composite material is used to inhibit bacteria and / or degrade dyes in dye-containing wastewater.
[0037] The specific method for the antibacterial application of magnetic fly ash / nano-silver composite material on solid plates is as follows: Colonies of *Escherichia coli*, *Staphylococcus aureus*, *Pseudomonas aeruginosa*, and *Bacillus subtilis* were picked and cultured on LB liquid medium (10 g / L beef peptone, 5 g / L yeast extract, 10 g / L sodium chloride) with shaking at 37°C. When the viable bacterial concentration reached 1.0 × 10⁻⁶... 8 At cfu / mL, 0.1 mL of Escherichia coli, Staphylococcus aureus, Pseudomonas aeruginosa, and Bacillus subtilis bacterial suspensions were respectively spread onto LB solid medium (beef peptone 10 g / L, yeast extract 5 g / L, sodium chloride 10 g / L, agar 20 g / L). Using a flame-sterilized perforator, 9.0 mm diameter holes were punched in the plates. Then, 0.05–0.2 g of the prepared fly ash / nano-silver composite material was filled into the holes. Finally, the plates were incubated at 37°C for 18 h, and the diameter of the inhibition zone was measured using a ruler.
[0038] The specific method for the antibacterial application of magnetic fly ash / nano-silver composite materials in water is as follows: Colonies of *Escherichia coli*, *Staphylococcus aureus*, *Pseudomonas aeruginosa*, and *Bacillus subtilis* were picked and cultured in LB liquid medium (5 g / L yeast extract, 10 g / L sodium chloride, 10 g / L beef peptone) at 37°C. When the viable bacterial concentration in the medium reached 1.0 × 10⁻⁶, the incubation period was determined. 8 When the concentration of cfu / mL was 0.2–1.0 g / L, the magnetic fly ash / nano-silver composite material prepared above was added, and the mixture was shaken and cultured for 4–18 h to obtain a bacterial suspension. Subsequently, 0.05–0.2 mL of the bacterial suspension was serially diluted with 0.9% sterile physiological saline, and the bacterial count was performed using the plate count method. The antibacterial rate of the magnetic fly ash / nano-silver composite material in water was calculated.
[0039] The specific method for dye degradation application is as follows: In a 250mL Erlenmeyer flask, add 100mL of methylene blue dye (50-150mg / L), 1-3mL of NaBH4 (0.2mol / L), and 25-75mg of magnetic fly ash / nano silver composite material, respectively. Place the flask on a magnetic stirrer at 30℃ and react. Take 2mL of sample every 5min to measure the concentration of residual methylene blue at 664nm and calculate the dye degradation rate.
[0040] Fly ash is the ash-like substance collected in combustion equipment after coal combustion. It is an industrial waste but also a potential resource, mainly composed of inorganic substances such as silicon dioxide, aluminum oxide, and iron oxide. Fly ash is widely available, inexpensive, porous, has a large specific surface area, and good adsorption properties. Its chemical properties are stable, and its inorganic components do not change significantly at high temperatures. Therefore, fly ash can be used as a carrier to uniformly distribute active silver ions in a stable form within the fly ash structure, helping to achieve uniform dispersion and slow release of silver ions. This overcomes the disadvantage of easy agglomeration of nano-silver, making it an excellent nanophase reactor. Nano-silver has a strong killing effect on various Gram-positive bacteria, Gram-negative bacteria, and fungi. The silver ions released from its surface can react with the cell membrane or internal biomolecules of pathogens, interfering with their biological activity and inhibiting their growth and reproduction. Furthermore, using sodium borohydride as a reducing agent, nano-silver can reduce and hydrogenate the azo bonds in azo dye molecules, generating corresponding amino compounds, thus achieving degradation. Furthermore, nano-silver is easy to synthesize and its surface properties can be effectively controlled, which is beneficial for its wide application in water treatment and antibacterial purposes. Although nano-silver can be used as an antibacterial agent and catalyst, there have been no studies to date on loading nano-silver into fly ash for application in bacterial dye wastewater.
[0041] Example 1
[0042] A method for preparing a magnetic fly ash / nano silver composite material, specifically including the following steps:
[0043] Step S1: Place 50g of fly ash (5000 mesh) in 20mL of 10wt% hydrochloric acid solution and stir. Stir at 90℃ for 1h, filter and wash until neutral, then dry to obtain acidified fly ash.
[0044] Step S2: Mix 200 mL of 0.12 mol / L ferric chloride solution and 200 mL of 0.05 mol / L ferrous sulfate solution to obtain a mixed solution. Add 20 g of acidified fly ash to the mixed solution, place it on a magnetic stirrer and heat it to 70 °C. Then add 1 mol / L sodium hydroxide solution to adjust the pH to 8-9. Then place the beaker in an ultrasonic cleaner and ultrasonically disperse for 30 min. After that, let it stand and age for 1 h. Filter and wash the precipitate until neutral, and then dry it to obtain magnetic fly ash.
[0045] Step S3: Soak 5g of magnetic fly ash in 100mL of 0.5g / L AgNO3 solution in the dark and stir continuously for 2h. Then add 0.2g of trisodium citrate dihydrate and stir continuously for 24h to carry out the reduction reaction to obtain nano-silver. Finally, filter and dry the magnetic fly ash containing nano-silver particles and place it in a tube furnace for calcination at a heating rate of 10℃ / min under an inert atmosphere. The calcination temperature is 250℃ and the calcination time is 2h. After natural cooling to room temperature, grind to obtain magnetic fly ash / nano-silver composite material.
[0046] The magnetic fly ash / nano silver composite material prepared in Example 1 was characterized and analyzed by SEM, such as... Figure 1 As shown. From Figure 1 It can be seen that fly ash presents as relatively regular spherical glass microspheres with smooth surfaces. After acidification and magnetic modification, it can open up pores and increase a large number of new micropores, which greatly increases its specific surface area. This means that it provides more contact sites for the loading of nano-silver.
[0047] The magnetic fly ash / nano silver composite material prepared in Example 1 was characterized by FT-IR, such as... Figure 2 As shown. From Figure 2 It can be seen from this that 3420cm -1 There is a relatively broad absorption peak around 1620 cm⁻¹, which is caused by the strong stretching vibration of OH. -1 and 1370cm -1 These are the -COO asymmetric stretching vibration and the CH stretching vibration, respectively; 1100cm -1 Both exhibit a strong absorption peak, which is related to the stretching vibration of the Si-O bond in fly ash. This indicates that the hydroxyl and carboxyl groups in trisodium citrate participate in the synthesis and stabilization of nano-silver, and that the hydroxyl groups can reduce Ag. + For Ag 0 The carboxyl group can react with Ag. + They combine to form a network and act as a stabilizer.
[0048] The magnetic fly ash / nano silver composite material prepared in Example 1 was characterized by XRD analysis, such as... Figure 3 As shown. From Figure 3It can be seen that a broad diffraction characteristic peak appears at approximately 25° 2θ, indicating the presence of a large amount of amorphous glass in the fly ash. These structural characteristics give fly ash high hydrophilicity, surface activity, and adsorption properties. The rightward shift after modification indicates an increase in diffraction angle, a decrease in interplanar spacing, and lattice defects. Seven characteristic peaks of Fe3O4 nanoparticles (2θ = 30.3°, 35.5°, 43.3°, 53.4°, 57.3°, 63.8°, and 74.2°) can be observed in magnetized fly ash, corresponding to the (220), (311), (400), (422), (511), and (440) crystal planes of the Fe3O4 standard spectrum, respectively. The relevant diffraction peaks show four small peaks at 38.1°, 44.5°, 64.3°, and 78.1°, corresponding to the (111), (200), (220), and (311) crystal planes of the standard spectrum of nanosilver, respectively, belonging to the face-centered cubic structure. The XRD pattern shows that the fly ash was successfully magnetized and loaded with nanosilver particles.
[0049] The magnetic fly ash / nano silver composite material prepared in Example 1 was subjected to magnetic separation, such as... Figure 4 As shown. From Figure 4 As can be seen, the magnetic sample settles to the bottom when left to stand in the aqueous system. When a magnet is placed on the tube wall, a large number of magnetic particles rapidly gather on the side where the magnet is placed, achieving in-situ separation of the solid and liquid phases. Therefore, the magnetic fly ash / nano-silver composite material prepared in this embodiment possesses this magnetic property, laying the foundation for the rapid recovery and reuse of the composite material in wastewater.
[0050] Examples 2 to 6
[0051] To investigate the optimal concentration range of the AgNO3 solution in step S3, all steps in Example 1 were identical to those in Example 1, except that the AgNO3 solution concentration varied within the range of 0.05–0.9 g / L. Examples 2–6 were thus obtained. The magnetic fly ash / nano-silver composite materials prepared in Examples 2–6 were subjected to solid-plate antibacterial experiments, and the test results are shown in Table 1.
[0052] Table 1. AgNO3 solution concentration and test results in Examples 1-6
[0053]
[0054] Table 1 shows that different AgNO3 solution concentrations exhibit varying antibacterial effects against four indicator bacteria (Escherichia coli, Staphylococcus aureus, Pseudomonas aeruginosa, and Bacillus subtilis). As the AgNO3 concentration increases to 0.5 g / L, the antibacterial effect of the magnetic fly ash / nano-silver composite material gradually increases, indicating that increasing the AgNO3 concentration promotes the formation of more nano-silver. However, when the concentration continues to increase to 0.9 g / L, the antibacterial effect shows a decreasing trend.
[0055] Examples 7 to 11
[0056] To investigate the optimal range of calcination temperature in step S3, all steps in Example 1 were identical to those in Example 1, except that the calcination temperature varied within the range of 150–400°C. Examples 7–11 were obtained. The magnetic fly ash / nano-silver composite materials prepared in Examples 7–11 were subjected to a solid plate antibacterial experiment, and the test results are shown in Table 2.
[0057] Table 2. Calcination temperature and test results in Examples 1, 7-11.
[0058]
[0059] Table 2 shows that the magnetic fly ash / nano-silver composite material exhibits certain antibacterial effects against *Escherichia coli*, *Staphylococcus aureus*, *Pseudomonas aeruginosa*, and *Bacillus subtilis*, with varying antibacterial effects depending on the calcination temperature. At a calcination temperature of 250℃, the antibacterial material showed the strongest antibacterial effect against the four indicator bacteria, with the most significant effect against *Pseudomonas aeruginosa*, reaching a maximum inhibition zone of 28 mm. However, as the calcination temperature was further increased to 400℃, the antibacterial effect gradually weakened. This may be related to its structural changes; with increasing calcination temperature, the nano-silver particle size gradually increases, the loading gradually decreases, and its antibacterial activity gradually declines.
[0060] Examples 12 to 16
[0061] To investigate the optimal range of calcination time in step S3, all steps in Example 1 were identical to those in Example 1, except that the calcination time varied within the range of 0.5–5 h. Examples 12–16 were obtained. The magnetic fly ash / nano-silver composite materials prepared in Examples 12–16 were subjected to solid plate antibacterial experiments, and the test results are shown in Table 3.
[0062] Table 3. Calcination time and test results in Examples 1, 12-16
[0063]
[0064] Table 3 shows that calcination time has a certain impact on the antibacterial effect of magnetic fly ash / nano-silver composite material. As the calcination time increases from 0.5 h to 2 h, the antibacterial effect of magnetic fly ash / nano-silver composite material against the four indicator bacteria gradually increases, and the antibacterial effect is the best at 2 h of calcination; when the calcination time is further extended to 5 h, the antibacterial effect gradually weakens.
[0065] Example 17
[0066] Application of magnetic fly ash / nano-silver composite material for antibacterial activity in water: Colonies of Escherichia coli, Staphylococcus aureus, Pseudomonas aeruginosa, and Bacillus subtilis were collected and cultured on LB liquid medium (5 g / L yeast extract, 10 g / L sodium chloride, 10 g / L beef peptone) at 37°C. The viable bacterial concentration was measured to be 1.0 × 10⁻⁶. 8 At a concentration of cfu / mL, 0.2 g / L of the magnetic fly ash / nano-silver composite material prepared in Example 1 was added, and the mixture was shaken and cultured for another 9 h to obtain a bacterial suspension. Subsequently, 0.1 mL of the bacterial suspension was serially diluted with 0.9% sterile physiological saline, and the bacterial count was performed using the plate count method. The calculated antibacterial rate of the magnetic fly ash / nano-silver composite material in water was all above 99.9%.
[0067] Example 18
[0068] Application of magnetic fly ash / nano-silver composite material in the degradation of dyes in water: 100 mL of methylene blue dye (100 mg / L), 2 mL of NaBH4 (0.2 mol / L), and 50 mg of magnetic fly ash / nano-silver composite material were added to a 250 mL Erlenmeyer flask. The flask was placed on a magnetic stirrer at 30 °C for reaction. 2 mL samples were taken every 5 min, and the residual methylene blue concentration was measured at 664 nm. The final degradation rate of methylene blue dye was calculated to be 99%.
[0069] Example 19
[0070] Application of the recyclability of magnetic fly ash / nano-silver composite materials: For catalysts, high activity alone is insufficient; they must maintain their initial activity over a period of time or possess the ability to reactivate after deactivation. To evaluate the recyclability of the magnetic fly ash / nano-silver composite materials, the material was separated using a magnet after each reaction and reused for antibacterial and dye degradation experiments. This process was repeated 10 times. After each reaction, the antibacterial rate and dye degradation rate in water were measured, revealing that the material's antibacterial and dye degradation activities were essentially unaffected. This was because the reaction temperature was mild under ambient conditions, and no solid products were precipitated on the active sites of the solid catalyst during the reaction.
[0071] In summary, the present invention is reasonably designed and has the following advantages:
[0072] (1) A highly active magnetic fly ash / nano silver composite material was prepared by loading nano silver onto a magnetically modified fly ash carrier. It has the dual function of killing common harmful bacteria in the environment (Escherichia coli, Staphylococcus aureus, Pseudomonas aeruginosa and Bacillus subtilis) and degrading azo dyes (methylene blue).
[0073] (2) The magnetic fly ash / nano silver composite material prepared by the present invention can be easily separated from the water environment by an external magnetic field, so as to realize the rapid recovery and recycling of the material.
[0074] (3) In addition, fly ash is a waste product of coal-fired power plants. Modifying it for dye degradation and antibacterial purposes is an economical and efficient way to realize the resource utilization and high-value utilization of fly ash.
[0075] (4) The preparation method of the present invention is simple and the preparation conditions are not harsh, which can realize large-scale production.
[0076] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, and not to limit them; although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art should understand that modifications can still be made to the technical solutions described in the foregoing embodiments, or equivalent substitutions can be made to some or all of the technical features; and these modifications or substitutions do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a magnetic fly ash / nano-silver composite material for inhibiting bacteria in dye-containing wastewater, characterized in that: Specifically, the steps include the following: Step S1: Place fly ash in hydrochloric acid solution and stir. Filter and wash until neutral, then dry to obtain acidified fly ash. Step S2: Add the acidified fly ash obtained in step S1 to a mixed solution composed of ferric chloride solution and ferrous sulfate solution and stir. After the magnetic stirrer is heated to 70°C, add 1 mol / L sodium hydroxide solution to adjust the pH to 8-9. Then place the beaker in an ultrasonic cleaner for ultrasonic dispersion for 30 min. After that, let it stand and age for 1 h. Filter and wash the precipitate until it is neutral and then dry it to obtain magnetic fly ash. Step S3: The magnetic fly ash obtained in step S2 is immersed in AgNO3 solution in the dark and stirred continuously at room temperature; then, the reducing agent trisodium citrate dihydrate is added and the mixture is stirred continuously to carry out a reduction reaction to obtain nano-silver; finally, the magnetic fly ash containing nano-silver particles is filtered, dried, and placed in a tube furnace under an inert atmosphere at 10°C. o The calcination was carried out at a heating rate of C / min, with a calcination temperature of 150–400℃ and a calcination time of 0.5–5 h. After natural cooling to room temperature, the magnetic fly ash / nano silver composite material was obtained by grinding.
2. The method for preparing a magnetic fly ash / nano-silver composite material for inhibiting bacteria in dye-containing wastewater according to claim 1, characterized in that: In step S1, the mass percentage of hydrochloric acid solution is 5-20%, the solid-liquid ratio of fly ash to hydrochloric acid solution is 1g:4mL, the stirring temperature is 90℃, and the stirring time is 1h.
3. The method for preparing a magnetic fly ash / nano-silver composite material for inhibiting bacteria in dye-containing wastewater according to claim 1, characterized in that: In step S2, ferric chloride solution and ferrous sulfate solution are mixed in a volume ratio of 1:1, wherein the concentration of ferric chloride solution is 0.12 mol / L and the concentration of ferrous sulfate solution is 0.05 mol / L.
4. The method for preparing a magnetic fly ash / nano-silver composite material for inhibiting bacteria in dye-containing wastewater according to claim 1, characterized in that: In step S2, the solid-liquid ratio of the acidified fly ash to the mixed solution is 1g:20mL.
5. The method for preparing a magnetic fly ash / nano-silver composite material for inhibiting bacteria in dye-containing wastewater according to claim 1, characterized in that: In step S3, the concentration of the AgNO3 solution is 0.05–0.9 g / L, and the solid-liquid ratio of the magnetic fly ash to the AgNO3 solution is 1 g: 20 mL.
6. The method for preparing a magnetic fly ash / nano-silver composite material for inhibiting bacteria in dye-containing wastewater according to claim 1, characterized in that: In step S3, the ratio of the mass of trisodium citrate dihydrate to the concentration of AgNO3 solution is 1:2.5, and the reduction reaction time is 24 h.
7. An application of a magnetic fly ash / nano-silver composite material, characterized in that: The magnetic fly ash / nano silver composite material is prepared by the preparation method according to any one of claims 1 to 6, and the magnetic fly ash / nano silver composite material is used to inhibit bacteria in dye wastewater containing bacteria.
Citation Information
Patent Citations
High-strength antibacterial PMMA plate and preparation method thereof
CN111234140A
Preparation method of magnetic fly ash / molybdenum disulfide composite material and application thereof
CN111250032A