Tcn composite material, method for preparing the same and use thereof

By preparing TTF/g-C₃N₄ composite materials, the problems of narrow spectral response and easy recombination of photogenerated carriers in the degradation of Rhodamine B by existing photocatalysts were solved, and efficient photocatalytic degradation effect over a wide pH range was achieved.

CN118454732BActive Publication Date: 2026-11-24TIANJIN UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310072132.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-07
Publication Date
2026-11-24
Estimated Expiration
2043-02-07

AI Technical Summary

Technical Problem

Existing inorganic semiconductor photocatalytic materials suffer from problems such as narrow solar spectrum response range, leaching of toxic metal ions, and easy photocorrosion and deactivation when photocatalytically degrading Rhodamine B. Graphite-phase carbon nitride (g-C₃N₄) materials, on the other hand, suffer from problems such as easy recombination of photogenerated carriers and insufficient light absorption.

Method used

TTF/g-C₃N₄ composite materials were prepared by solvent evaporation. The synergistic effect of TTF and g-C₃N₄ was utilized to form TCN composite materials for photocatalytic degradation of Rhodamine B.

Benefits of technology

It achieves efficient degradation of Rhodamine B, especially maintaining high degradation efficiency in the range of strong acid to weak base (pH=1~9), significantly improving photocatalytic performance and broadening the applicable pH range.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118454732B_ABST
    Figure CN118454732B_ABST
Patent Text Reader

Abstract

This invention discloses a TCN composite material, its preparation method, and its application. The preparation method includes the following steps: uniformly dispersing tetrathionyl fulvalene and g-C3N4 in a solvent to obtain solution A, wherein the ratio of TTF to g-C3N4 by mass is (0.5-30):100; heating solution A at 40-60°C for 0.5-2 hours under stirring conditions, and then thoroughly drying to obtain the TCN composite material. Compared with monomeric TTF and g-C3N4 catalysts, the TCN composite material of this invention exhibits superior catalytic activity, achieving highly efficient removal of RhB. The TCN composite material of this invention maintains high degradation efficiency in the range from strong acid to weak base.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the technical field of Rhodamine B degradation materials, specifically relating to a TCN composite material, its preparation method, and its application. Background Technology

[0002] Rhodamine B (RhB), a cationic basic dye, is commonly used in fluorescent probes and cell staining experiments, and is also widely used in the production of colored glass and fireworks in manufacturing. Due to its complex chemical structure, it is chemically stable and difficult to biodegrade. When discharged into the environment through wastewater, it seriously affects the stability of aquatic ecosystems and endangers human health. Therefore, there is an urgent need to develop efficient and environmentally friendly methods to remove RhB from the environment.

[0003] Solar energy, as the most primitive and cleanest energy source on Earth, has attracted widespread attention from scholars. Photocatalytic oxidation using solar energy holds immense potential for alleviating the severe energy crisis and addressing prominent environmental problems. The generation of various active substances in the photocatalytic system is key to the oxidative degradation of pollutants. Among these, O2 participating in the reaction can be converted into hydroxyl radicals (H2) by the photocatalyst. + and e - Oxidized or reduced to O2 - H2O2, ·OH and 1 O2 and other reactive species. Under the action of reactive substances, organic pollutants can be deeply oxidized into fragment molecules, until they are transformed into harmless products, such as small molecules like CO2, H2O and N2.

[0004] Currently, a large number of inorganic semiconductor photocatalytic materials have been developed for photocatalysis. However, these materials still suffer from problems such as narrow solar spectral response range, leaching of toxic metal ions, and easy photocorrosion deactivation. Therefore, the development of novel and efficient metal-free organometallic semiconductor (OSC) photocatalytic materials is a research hotspot. Graphitic carbon nitride (g-C3N4), as a metal-free, highly stable organic polymer semiconductor material, is inexpensive, easy to prepare, and has good solar energy utilization capabilities, and has been widely used in the field of photocatalysis. However, it still has problems such as easy recombination of photogenerated carriers and insufficient light absorption, and it is urgent to modify it through heterostructure construction and elemental doping to improve its photocatalytic performance. Summary of the Invention

[0005] To address the shortcomings of existing technologies, the present invention aims to provide a method for preparing a TCN composite material (TTF / g-C3N4), which obtains a TCN composite material in which TTF (tetrathiofulvalene) and g-C3N4 have a synergistic effect through solvent evaporation.

[0006] Another object of the present invention is to provide a TCN composite material obtained by the above preparation method.

[0007] Another objective of this invention is to provide the application of the above-mentioned TCN composite material as a catalyst in the photocatalytic degradation of Rhodamine B (RhB). Under conditions of external light irradiation and continuous oxygen exposure, the TCN composite material achieves effective degradation of RhB.

[0008] The objective of this invention is achieved through the following technical solution.

[0009] A method for preparing a TCN composite material includes the following steps:

[0010] 1) TTF (tetrathiofulvalene) and g-C3N4 are uniformly dispersed in a solvent to obtain solution A, wherein the ratio of TTF to g-C3N4 by mass parts is (0.5~30):100;

[0011] In step 1), the ratio of TTF to g-C3N4 by mass parts is (4-15):100, preferably (4-13):100.

[0012] In step 1), the method for obtaining g-C3N4 is as follows: urea is calcined at 530-550°C for 2-2.5 hours in an air atmosphere to obtain g-C3N4.

[0013] In step 1), the method for uniformly dispersing TTF and g-C3N4 in the solvent is as follows: mix TTF, g-C3N4 and solvent, and sonicate for at least 20 minutes.

[0014] In the above technical solution, urea is released from room temperature at a rate of 2–2.5 °C / min. -1 The temperature is increased to 530–550℃ and calcined at 530–550℃ for 2–2.5 hours.

[0015] In step 1), the solvent is tetrahydrofuran.

[0016] In step 1), the ratio of the mass fraction of g-C3N4 to the volume fraction of the solvent is (30-50):(5-8.5), where the mass fraction is in mg and the volume fraction is in mL.

[0017] 2) Under stirring conditions, the solution A is heated at 40-60°C for 0.5-2 hours and dried thoroughly to obtain the TCN composite material.

[0018] In step 2), the thorough drying is achieved by maintaining the temperature at 60–70°C for 24–48 hours.

[0019] The TCN composite material obtained by the above preparation method.

[0020] The above-mentioned TCN composite material is used as a catalyst in the photocatalytic degradation of Rhodamine B.

[0021] In the above technical solution, TCN composite material is added to wastewater containing Rhodamine B, oxygen is introduced, and after adsorption-desorption equilibrium is reached under dark conditions, photocatalytic degradation is carried out under light.

[0022] In the above technical solution, the pH of the wastewater containing Rhodamine B is 1 to 10.

[0023] In the above technical solution, oxygen is introduced under stirring conditions at a rate of 100–120 mL / min. -1 .

[0024] In the above technical solution, the time to reach adsorption-desorption equilibrium is 30 to 60 minutes.

[0025] In the above technical solution, the light intensity of the illumination is 100-150 mW·cm. -1 .

[0026] In the above technical solution, the ratio of the mass fraction of the TCN composite material to the volume fraction of the wastewater is (3-20):(20-150), where the mass fraction is in mg and the volume fraction is in mL.

[0027] In the above technical solution, the concentration of RhB in the wastewater is 5–10 mg·L⁻¹. -1 .

[0028] Compared with the prior art, the beneficial effects of the present invention are:

[0029] 1. Compared with monomeric TTF and g-C3N4 catalysts, the TCN composite material of the present invention exhibits superior catalytic activity, achieving efficient removal of RhB.

[0030] 2. The TCN composite material of the present invention maintains a high degradation efficiency in the range of strong acid to weak base (pH=1 to 9). Attached Figure Description

[0031] Figure 1 The degradation efficiency of RhB by the TCN composite materials obtained in Examples 1-4 is shown.

[0032] Figure 2 The degradation efficiency of RhB in Examples 9 and 14-18;

[0033] Figure 3 The degradation efficiency of RhB in Examples 9, 12, 13 and 19;

[0034] Figure 4 The degradation efficiency of RhB in Examples 9, 20 and 21;

[0035] Figure 5 The photocurrent response of the TCN composite material prepared in Example 2 and the g-C3N4 catalyst prepared in Example 5;

[0036] Figure 6 Electrochemical impedance of the TCN composite material prepared in Example 2 and the g-C3N4 catalyst prepared in Example 5;

[0037] Figure 7 Transient fluorescence spectroscopy tests were performed on the TCN composite material prepared in Example 2 and the g-C3N4 catalyst prepared in Example 5.

[0038] Figure 8 The UV-Vis diffuse reflectance spectra of the TCN composite material prepared in Example 2 and the g-C3N4 catalyst prepared in Example 5 are shown. Detailed Implementation

[0039] The technical solution of the present invention will be further described below with reference to specific embodiments.

[0040] The purity and manufacturers of the pharmaceuticals involved in the following examples are as follows:

[0041]

[0042]

[0043] The models and manufacturers of the instruments involved in the following embodiments are as follows:

[0044]

[0045] Examples 1-4

[0046] A method for preparing a TCN composite material includes the following steps:

[0047] 1) Under air atmosphere, urea is heated from room temperature (20-25℃) at a rate of 2.5℃·min. -1 The temperature was increased to 550℃ and calcined at 550℃ for 2 hours to obtain g-C3N4. X mg TTF (tetrathiofulvalene), 30 mg g-C3N4 and 5 mL solvent were mixed and sonicated for 30 min to obtain solution A, wherein the solvent was tetrahydrofuran;

[0048] 2) Under stirring conditions, solution A was heated on a heating plate at 60°C for 1 hour, and then placed in a forced-air drying oven at 60°C for 48 hours to allow it to dry completely, thus obtaining the TCN composite material.

[0049] The values ​​of X are shown in Table 1.

[0050] Table 1

[0051]

[0052] Example 5

[0053] A method for preparing a g-C3N4 catalyst includes the following steps:

[0054] Weigh 25g of urea into a covered crucible, and heat it in a muffle furnace under air atmosphere from room temperature (20-25℃) at a rate of 2.5℃·min. -1 The temperature was increased to 550℃ and calcined at 550℃ for 2 hours, then naturally cooled to room temperature (20-25℃) to obtain g-C3N4 catalyst.

[0055] Example 6

[0056] A TTF catalyst, purchased from Beijing Bailingwei Technology Co., Ltd., has the following specifications:

[0057] Table 2

[0058] Drug Name Tetrathione English name Tetrathiafulvalene (TTF) Molecular formula <![CDATA[C6H4S4]]> Specification 1G purity 98.5% CAS number 31366-25-3

[0059] Example 7

[0060] The photocatalytic degradation of RhB was carried out in a 100 mL beaker at room temperature of 20–25 °C. The photocatalytic degradation conditions were as follows: 50 mL of RhB (Rhodamine B) aqueous solution was placed in the 100 mL beaker as simulated RhB wastewater, and the concentration of RhB in the simulated RhB wastewater was 10 mg·L⁻¹. -1 The simulated RhB wastewater pH value was 0.5 mol·L⁻¹ -1 NaOH aqueous solution or 0.5 mol·L⁻¹ -1 The pH of the simulated RhB wastewater was adjusted using an aqueous H2SO4 solution to achieve the initial pH shown in Table 3. O2 was then introduced into the simulated RhB wastewater via a gas delivery tube at a flow rate of 100 mL / min. -1 The mixture was stirred continuously in the dark for 30 minutes to reach adsorption-desorption equilibrium. Then, it was illuminated with a xenon lamp (vertical top illumination) equipped with an ultraviolet filter, providing visible light (wavelength > 420 nm) at an intensity of 100 mW·cm². -1 5 mg of catalyst was added to simulated RhB wastewater to conduct a photocatalytic degradation experiment of RhB. During the degradation process, the mixture was continuously stirred to ensure that the catalyst was uniformly dispersed in the simulated RhB wastewater. The catalyst was one of the TCN composite material in Examples 1-4, the g-C3N4 catalyst obtained in Example 5, and the TTF catalyst in Example 6. The types of catalysts added are shown in Table 3.

[0061] Table 3

[0062] Example number Simulated RhB wastewater reaction initial pH catalyst Example 8 7 Example 1 Example 9 7 Example 2 Example 10 7 Example 3 Example 11 7 Example 4 Example 12 7 Example 5 Example 13 7 Example 6 Example 14 1 Example 2 Example 15 3 Example 2 Example 16 5 Example 2 Example 17 9 Example 2 Example 18 10 Example 2

[0063] Example 19

[0064] At room temperature (20–25°C), a photocatalytic degradation experiment was conducted on simulated RhB wastewater using a mechanical mixture of TTF and g-C3N4 in a 100 mL beaker. The photocatalytic degradation conditions were as follows: 50 mL of RhB (Rhodamine B) aqueous solution was placed in a 100 mL beaker as simulated RhB wastewater, and the RhB concentration in the simulated RhB wastewater was 10 mg·L⁻¹. -1 The simulated RhB wastewater pH value was 0.5 mol·L⁻¹ -1 NaOH aqueous solution or 0.5 mol·L⁻¹ -1 The pH of the H2SO4 aqueous solution was adjusted to 7. O2 was then introduced into the simulated RhB wastewater via a gas delivery tube at a flow rate of 100 mL / min. -1 The mixture was stirred continuously in the dark for 30 minutes to reach adsorption-desorption equilibrium. Then, it was illuminated with a xenon lamp equipped with an ultraviolet filter, providing visible light (wavelength > 420 nm) at an intensity of 100 mW·cm². -1 4.75 mg of the g-C3N4 catalyst obtained in Example 5 and 0.25 mg of the TTF catalyst in Example 6 were added to simulated RhB wastewater to conduct a photocatalytic degradation experiment of RhB. During the degradation process, the mixture was continuously stirred to ensure that the catalyst was uniformly dispersed in the simulated RhB wastewater.

[0065] Example 20

[0066] The photocatalytic self-degradation experiment of RhB was carried out in a 100 mL beaker at room temperature of 20–25 °C. The photocatalytic self-degradation conditions were as follows: 50 mL of RhB (Rhodamine B) aqueous solution was placed in the 100 mL beaker as simulated RhB wastewater, and the concentration of RhB in the simulated RhB wastewater was 10 mg·L⁻¹. -1 The simulated RhB wastewater pH value was 0.5 mol·L⁻¹ -1 NaOH aqueous solution or 0.5 mol·L⁻¹ -1 The pH of the H2SO4 aqueous solution was adjusted to 7. O2 was then introduced into the simulated RhB wastewater via a gas delivery tube at a flow rate of 100 mL / min. -1 After stirring continuously in the dark for 30 minutes, the mixture was then illuminated with a xenon lamp equipped with an ultraviolet filter, providing visible light (wavelength > 420 nm) at an intensity of 100 mW·cm². -1 .

[0067] Example 21

[0068] At room temperature of 20–25°C, a dark reaction degradation experiment was conducted on simulated RhB wastewater using the TCN composite material prepared in Example 2 in a 100 mL beaker. The experimental conditions were as follows: 50 mL of RhB (Rhodamine B) aqueous solution was placed in a 100 mL beaker as simulated RhB wastewater, and the RhB concentration in the simulated RhB wastewater was 10 mg·L⁻¹. -1 The simulated RhB wastewater pH value was 0.5 mol·L⁻¹ -1 NaOH aqueous solution or 0.5 mol·L⁻¹ -1 The pH of the H2SO4 aqueous solution was adjusted to 7. O2 was then introduced into the simulated RhB wastewater via a gas delivery tube at a flow rate of 100 mL / min. -1 5 mg of the TCN composite material prepared in Example 2 was added to simulated RhB wastewater and the mixture was continuously stirred and reacted in the dark.

[0069] Examples 8-11 illustrate the photocatalytic degradation of RhB using the TCN composite materials prepared in Examples 1-4, with the following results: Figure 1 As shown, the TCN composite materials prepared in Examples 1-4 exhibited significant differences in their effect on RhB degradation efficiency. The TCN-1 prepared in Example 1, TCN-5 prepared in Example 2, TCN-10 prepared in Example 3, and TCN-15 prepared in Example 4 achieved RhB degradation efficiencies of 76.9%, 96.2%, 92.6%, and 82.5% respectively after 60 min. With increasing TTF doping concentration, the degradation efficiency first increased and then decreased. The TCN composite material prepared in Example 2 demonstrated excellent catalytic performance; the entire photocatalytic degradation process was significantly faster than that of the TCN composite materials prepared in Examples 1, 3, and 4, significantly improving the RhB degradation efficiency. Therefore, the TCN composite material prepared in Example 2 was selected as the optimal catalyst for subsequent studies.

[0070] Examples 9 and 14-18 illustrate the photocatalytic degradation of RhB by the TCN composite material prepared in Example 2 under different pH conditions. The results are as follows: Figure 2As shown, the RhB degradation efficiency gradually increased within the first 30 minutes as the pH value was adjusted from 10 to 1, indicating that an acidic environment is more conducive to RhB degradation. At 60 minutes, the RhB degradation efficiencies reached 97.8%, 96.8%, 96.6%, 96.2%, 92.4%, and 68.1% at pH = 1, 3, 5, 7, 9, and 10, respectively. This demonstrates that the TCN composite material prepared in Example 2 has good applicability within the pH range of 1-9 (i.e., from strong acid to weak base), greatly broadening the pH range for photocatalytic degradation of pollutants. A more alkaline environment (pH = 10) is unfavorable for H2O2 production, leading to a rapid decrease in degradation efficiency. Considering that the pH range of solutions in actual water treatment tends to be neutral, pH = 7 was chosen as the initial pH value of the pollutant solution for subsequent studies.

[0071] Examples 9, 12, 13, and 19 illustrate the photocatalytic degradation of RhB using different catalysts, and the results are as follows: Figure 3 As shown, the degradation efficiencies of the g-C3N4 catalyst prepared in Example 5 and the TTF catalyst represented in Example 6 for RhB at 60 min were 32.0% and 49.8%, respectively. However, under the catalytic action of the TCN composite material prepared in Example 2, RhB was rapidly degraded, with a final degradation efficiency of 96.2% (60 min), which was 64.2% and 46.4% higher than the degradation efficiencies of the g-C3N4 catalyst prepared in Example 5 and the TTF catalyst represented in Example 6, respectively. This indicates a synergistic effect between the TTF catalyst and g-C3N4, significantly enhancing the photocatalytic performance of the TCN composite material prepared in Example 2, thereby promoting the degradation of RhB.

[0072] Examples 9 and 21 show the degradation of RhB by the TCN composite material prepared in Example 2 under different conditions. The results are as follows: Figure 4 As shown. Stirring in the dark for 1 hour did not degrade RhB, indicating that the physical adsorption between the TCN composite material prepared in Example 2 and RhB was relatively weak. However, under visible light, the catalytic activity of the TCN composite material prepared in Example 2 was photoexcited, causing RhB to degrade rapidly within 40 minutes, and then gradually reach equilibrium. The final degradation efficiency reached 96.2% (60 minutes), and the pollutant solution changed from purplish-red to colorless. Light, as an indispensable external condition, indicates that the TCN composite material prepared in Example 2 is more suitable for photocatalytic systems. Comparing Examples 9 and 20, in the photocatalytic self-degradation experiment of RhB without the TCN composite material, the self-degradation efficiency of RhB under visible light was only 1.4%, indicating that the presence of the TCN composite material accelerated the degradation of RhB. Therefore, the TCN composite material prepared in Example 2 has been successfully applied to the field of photocatalytic degradation of pollutants.

[0073] Example 22

[0074] The photocurrent response of the TCN composite material prepared in Example 2 and the g-C3N4 catalyst prepared in Example 5 was tested. The specific procedures for the photocurrent response test were as follows: an electrochemical workstation (Chenhua CHI 660D) was used, and a xenon lamp was used to provide visible light illumination. A three-electrode system was employed, with a platinum sheet as the auxiliary electrode and a saturated calomel electrode as the reference electrode. The working electrode was prepared by adding 20 mg of the catalyst (either the TCN composite material prepared in Example 2 or the g-C3N4 catalyst prepared in Example 5) to 1 mL of ethanol, followed by the addition of 20 μL of naphthol. The mixture was sonicated for 30 min to uniformly disperse the catalyst in the solution. The dispersed solution was then uniformly dropped onto the conductive surface of an FTO glass plate and allowed to air dry for 12 h to obtain the working electrode.

[0075] A three-electrode system was used, with a concentration of 0.05 mol·L⁻¹. -1 The photocurrent response was tested using an aqueous solution of Na2SO4 as the electrolyte solution, and the results are as follows: Figure 5 As shown, the g-C3N4 catalyst prepared in Example 5 and the TCN composite material prepared in Example 2 exhibited different photoresponses. When illumination began, the photocurrent density of both catalysts increased rapidly, indicating the generation and effective separation of photogenerated carriers under illumination. After the light was turned off, the photocurrent density decreased rapidly. The TCN composite material prepared in Example 2 showed a higher photocurrent response, with a maximum photocurrent density reaching 0.24 μA·cm⁻¹. -2 Experiments show that TTF effectively modifies g-C3N4, promotes the effective separation of photogenerated electron-hole pairs, and enables the TCN composite material prepared in Example 2 to obtain better optical properties, which is more conducive to the photocatalytic reaction.

[0076] Example 23

[0077] Electrochemical impedance spectroscopy (EIS) tests were performed on the TCN composite material prepared in Example 2 and the g-C3N4 catalyst prepared in Example 5. The specific procedures for the EIS test were as follows: an electrochemical workstation (Chenhua CHI 660D) was used, and a xenon lamp was used to provide visible light illumination. A three-electrode system was employed, with a platinum sheet as the auxiliary electrode and a saturated calomel electrode as the reference electrode. The working electrode was prepared by adding 2 mg of the TCN composite material prepared in Example 2 or the g-C3N4 catalyst prepared in Example 5 to 2 mL of ethanol, followed by the addition of 20 μL of naphthol. The mixture was sonicated for 30 min to ensure uniform dispersion of the catalyst. The dispersed solution was then dropped onto a glassy carbon electrode and allowed to air dry for 20 min to obtain the working electrode.

[0078] A three-electrode system was used, with a concentration of 0.05 mol·L⁻¹. -1Electrochemical impedance spectroscopy was performed using an aqueous solution of Na₂SO₄ as the electrolyte solution, and the results are as follows: Figure 6 As shown, a smaller radius of curvature indicates lower resistance to interfacial charge transfer, which is more conducive to charge separation. Compared with the g-C3N4 catalyst prepared in Example 5, the TCN composite material prepared in Example 2 has a smaller curvature, indicating lower resistance to interfacial charge transfer and facilitating rapid interfacial charge transfer. Therefore, the photocatalytic performance of the TCN composite material is superior to that of g-C3N4.

[0079] Example 24

[0080] Transient fluorescence spectroscopy was performed on the TCN composite material prepared in Example 2 and the g-C3N4 catalyst prepared in Example 5 using a fluorescence spectrometer (F-7000) to characterize the separation and recombination of photogenerated carriers in the catalysts. The results are as follows: Figure 7 As shown, both the g-C3N4 catalyst prepared in Example 5 and the TCN composite material prepared in Example 2 exhibit transient fluorescence emission peaks within the wavelength range of 400–600 nm. The broad peak at 440 nm of the g-C3N4 catalyst prepared in Example 5 is attributed to intrinsic LUMO to HOMO excitation, while the shoulder peak at 460 nm is the fluorescence emission peak generated after the recombination of photogenerated electron-hole pairs. The transient fluorescence emission peak intensity of the TCN composite material prepared in Example 2 is significantly reduced, confirming a significant improvement in its photogenerated carrier separation rate. This indicates that TTF successfully modifies g-C3N4, and the resulting TCN composite material prepared in Example 2 possesses high photocatalytic performance.

[0081] Example 25

[0082] The UV-Vis diffuse reflectance (UV-vis DRS) of the TCN composite material prepared in Example 2 and the g-C3N4 catalyst prepared in Example 5 were measured using a UV-Vis near-infrared spectrophotometer (UV-3600Plus). The results are as follows: Figure 8 As shown. The TCN composite material prepared in Example 2 and the g-C3N4 catalyst prepared in Example 5 both exhibit good light absorption in the 200-420 nm range, with slight differences at the absorption boundary. The band gap widths of the TCN composite material prepared in Example 2 and the g-C3N4 catalyst prepared in Example 5 were analyzed using the Kubelka-Munk function formula (1), and the results are shown below. Figure 8 As shown in the illustration.

[0083] αhν = A (hν - Eg) n / 2 (1)

[0084] Among them, E gThe bandgap width is represented by α, A is a constant, and ν, h, and α are the frequency, Planck's constant, and absorption coefficient, respectively. The n values ​​for direct bandgap and indirect bandgap semiconductors are 1 and 4, respectively. The TCN composite material prepared in Example 2 and the g-C3N4 prepared in Example 5 are both indirect bandgap semiconductors, therefore n is taken as 4. (See the illustration (αhν)) 2 / n The band gap width E of the TCN composite material prepared in Example 2 and the g-C3N4 prepared in Example 5 was obtained from the x-axis intercept of the -hν curve. g The values ​​are 2.85 and 2.83 eV, respectively.

[0085] The present invention has been described above by way of example. It should be noted that any simple modifications, alterations or other equivalent substitutions that can be made by those skilled in the art without creative effort without departing from the core of the present invention fall within the protection scope of the present invention.

Claims

1. The application of a TCN composite material as a catalyst in the photocatalytic degradation of Rhodamine B, characterized in that, TCN composite material was added to wastewater containing Rhodamine B, oxygen was introduced, and after adsorption-desorption equilibrium was reached under dark conditions, photocatalytic degradation was carried out under light. The pH of the wastewater containing Rhodamine B was 1-9, and the light intensity was 100 mW·cm². -1 Oxygen is introduced under stirring conditions at a rate of 100–120 mL / min. -1 ; The preparation method of the TCN composite material includes the following steps: 1) Tetrathiofulvalene and g-C3N4 are uniformly dispersed in a solvent to obtain solution A, wherein the ratio of tetrathiofulvalene to g-C3N4 by mass is 5.27:100; 2) Under stirring conditions, the solution A is heated at 40~60 ℃ for 0.5~2 h and dried thoroughly to obtain the TCN composite material.

2. The application according to claim 1, characterized in that, In step 1), the method for uniformly dispersing tetrathione and g-C3N4 in the solvent is as follows: mix tetrathione, g-C3N4 and solvent, and sonicate for at least 20 min.

3. The application according to claim 1, characterized in that, In step 1), the solvent is tetrahydrofuran.

4. The application according to claim 1, characterized in that, In step 1), the ratio of the mass fraction of g-C3N4 to the volume fraction of the solvent is (30~50):(5~8.5), where the mass fraction is in mg and the volume fraction is in mL.

5. The application according to claim 1, characterized in that, In step 2), the thorough drying is achieved by maintaining the temperature at 60-70°C for 24-48 hours.

6. The application according to claim 1, characterized in that, The time to reach adsorption-desorption equilibrium is 30~60 min.

7. The application according to claim 1, characterized in that, The ratio of the mass fraction of the TCN composite material to the volume fraction of the wastewater is (3~20):(20~150), where the mass fraction is in mg and the volume fraction is in mL.

8. The application according to claim 1, characterized in that, The concentration of RhB in the wastewater was 5-10 mg / L. -1 .

Citation Information

Patent Citations

  • Organic coated composite semiconductor material and preparation method and application thereof

    CN115672397A