A porous carbon material and a preparation method and application thereof
Porous carbon materials were prepared by high-temperature carbonization reaction of powder catalyst supported on heavy oil, which solved the problems of pore size uniformity and poor conductivity, and enabled the widespread application of porous carbon materials in energy storage and separation and purification.
Patent Information
- Application Number
- CN202410435934.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-11
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-04-11
AI Technical Summary
Existing porous carbon materials have poor pore size uniformity and electrical conductivity, making it difficult to achieve controllable pore size adjustment, which limits their application in energy storage and separation and purification.
Using heavy oil as a carbon source, porous carbon materials are prepared by loading heavy oil onto the surface of powder catalysts and performing high-temperature carbonization reactions under an inert atmosphere, combined with acid washing and purification treatment. The specific surface area and pore size can be flexibly adjusted.
The prepared porous carbon material has a large specific surface area, uniform pore size distribution, excellent conductivity and stability, and is suitable for purification adsorption materials, catalyst supports and electrode materials.
Smart Images

Figure CN118458737B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the fields of materials science and electrochemical technology, specifically relating to a porous carbon material, its preparation method, and its application. Background Technology
[0002] Porous carbon materials are carbon materials with high specific surface area and highly developed pore structure. Their pore size distribution can be controlled according to actual needs, ranging from nanometer to micrometer scales. Porous carbon materials have advantages such as high chemical stability, low cost, narrow pore size distribution, and good electrical conductivity. The presence of the pore structure helps enhance the adsorption capacity of carbon materials and increase their specific surface area. Therefore, porous carbon materials can be applied in fields such as energy storage, separation and purification, and chromatographic analysis.
[0003] There are many raw materials for preparing porous carbon materials, with peat, lignite, wood scraps, pulp waste, and waste plastics being the main precursors. These raw materials are inexpensive, but the resulting porous carbon materials have poor performance. Porous carbon materials prepared using synthetic resins as precursors exhibit excellent performance but are more expensive. In contrast, novel porous carbon materials prepared using heavy oils such as asphalt and residual oil as carbon source precursors offer advantages such as low cost, excellent performance, high carbon content, and the ability to be mass-produced.
[0004] Currently, the most studied method for synthesizing porous carbon materials is the activation method. Porous carbon materials prepared by the activation method have advantages such as a large number of micropores and a large specific surface area. However, they also have some disadvantages, such as small pore size, weak conductivity, and easy collapse of the pore structure. Therefore, this method has certain limitations in application, namely, it is difficult to achieve the requirement of uniform and controllable pore size. Therefore, a new technology is urgently needed to overcome the above-mentioned shortcomings and deficiencies and achieve the controllable preparation of porous carbon materials. Summary of the Invention
[0005] In view of this, the present invention aims to provide a method for preparing porous carbon materials from heavy oil, which allows for flexible adjustment of the morphology, structure, specific surface area and pore size of the porous carbon materials.
[0006] This invention provides a method for preparing porous carbon materials. The method involves loading heavy oil onto the surface of a powdered catalyst, performing a high-temperature carbonization reaction under an inert atmosphere, and after the reaction is complete, removing the reaction product for acid washing and purification, followed by filtration and drying to obtain the porous carbon material.
[0007] Preferably, the preparation method is as follows: the powdered catalyst is impregnated and dispersed in heavy oil, and then ultrasonically treated to obtain a heavy oil / catalyst composite; then the heavy oil / catalyst composite is placed in a ceramic boat and placed in a horizontal tube furnace, and heated at 5°C for 1 minute under an inert atmosphere. -1 -10℃min-1 The heating rate is increased to 700℃-900℃, and the reaction is carried out under normal pressure for 50-80 minutes. After the reaction is completed, the mixture is cooled to room temperature, the black substance is taken out, the catalyst is removed by acid washing, and then washed and dried. The black substance obtained is the porous carbon material.
[0008] Preferably, the preparation method is as follows: placing the powdered catalyst in a rotating bed reactor, and under an inert atmosphere, at 5°C for 1 minute... -1 -10℃min -1 The heating rate was increased to 700℃-900℃, and then the gasified heavy oil was introduced into a rotating bed reactor. The reaction was carried out at atmospheric pressure and constant temperature for 20-30 minutes. After the reaction was completed, it was cooled to room temperature, and the resulting black substance was removed. The catalyst was removed by acid washing, and the mixture was washed and dried to obtain porous carbon material. Sufficient gas-solid contact between the catalyst and the gasified carbon source ensured heat and mass transfer between the gas and solid phases. Under suitable carbonization temperature, homogeneous carbon layer growth at the catalyst interface was achieved more effectively in a shorter time.
[0009] Preferably, in the above preparation method, the weight ratio of heavy oil to powdered catalyst is 10:(5-100).
[0010] Preferably, in the above preparation method, the weight ratio of heavy oil to powdered catalyst is 10:(15-50).
[0011] Preferably, in the above preparation method, the heavy oil includes one or a combination of several of the following: coal tar, ethylene tar, coal pitch, petroleum pitch, deasphalted oil, vacuum wax oil, vacuum residue, petroleum coke, waste tire oil, and waste plastic oil.
[0012] Preferably, in the above preparation method, the powder catalyst includes one or more of copper oxide, aluminum oxide, calcium oxide, ferric oxide, and silicon dioxide.
[0013] Preferably, in the above preparation method, the inert atmosphere includes one or a combination of nitrogen, helium and argon.
[0014] The present invention also provides a porous carbon material prepared by the above preparation method, wherein the porous carbon material has a specific surface area of 1000-1500 m². 2 g -1 The pore size distribution is 0.5-80 nm, and the iodine value is greater than 1350 mg g. -1 .
[0015] The present invention also provides an application of the above-mentioned porous carbon material in the preparation of purification adsorption materials, catalyst supports and electrode materials.
[0016] Compared with the prior art, the present invention uses heavy oil as a carbon source. By uniformly loading heavy oil onto a catalyst and then performing a high-temperature carbonization reaction, a homogeneous carbon layer is grown at the catalyst interface to obtain a porous carbon material. Furthermore, by adjusting the material ratio of gaseous carbon to catalyst and the reaction parameters (temperature, time), the specific surface area and pore size of the porous carbon material can be flexibly adjusted. Attached Figure Description
[0017] Figure 1 This is a scanning electron microscope (SEM) image of the porous carbon material prepared in Example 1 of this invention. Figure 2 This is a transmission electron microscope (TEM) image of the porous carbon material prepared in Example 1 of this invention. Figure 3 This is a scanning electron microscope (SEM) image of the porous carbon material prepared in Example 3 of the present invention. Figure 4 The rate performance diagram of the porous carbon electrode prepared in Example 3 of this invention; Figure 5 The image shows the cyclic voltammetry curve of the porous carbon electrode prepared in Example 3 of this invention. Detailed Implementation
[0018] To provide a clearer understanding of the technical features, objectives, and beneficial effects of the present invention, the technical solution of the present invention will now be described in detail with reference to the following specific embodiments, but this should not be construed as limiting the scope of implementation of the present invention.
[0019] Example 1 This embodiment provides a method for preparing porous carbon materials, wherein the preparation method includes the following specific steps: placing 30 g of powdered magnesium oxide catalyst in a rotating bed reactor, and under an argon atmosphere, at 5 °C for min... -1 The heating rate was increased to 800 °C, and then 20 g of ethylene tar was gasified at 180 °C. The gasified ethylene tar was then fed into a rotating bed reactor for 25 minutes at atmospheric pressure. After the reaction was completed, the mixture was cooled to room temperature, and the resulting black substance was removed. The catalyst was removed by acid washing, and the mixture was washed and dried. The resulting black substance is the porous carbon material.
[0020] The porous carbon material prepared in Example 1 was subjected to scanning electron microscopy (SEM) testing, such as... Figure 1 As shown, the porous carbon material exhibits a layered morphological structure. Transmission electron microscopy (TEM) analysis was performed on the prepared porous carbon material, as shown... Figure 2 As shown, the porous carbon material has 1-2 layers, indicating that it has a good thin-layer structure.
[0021] The specific surface area of the porous carbon material was measured to be 1650 m².2 g -1 The iodine value of the porous carbon material was tested and found to be 1365 mg g. -1 When this porous carbon material is used as the anode material for lithium-ion batteries, the capacity is 525 mAh g. -1 When this porous carbon material is used as an electrode material for a supercapacitor, the capacitance is 255 F g. -1 .
[0022] Example 2 This embodiment provides a method for preparing porous carbon materials, wherein the preparation method includes the following specific steps: 30 g of powdered magnesium oxide catalyst is added to 20 g of ethylene tar for impregnation, followed by ultrasonication for 10 minutes. The resulting mixture is placed in a ceramic boat and then placed in a horizontal tube furnace, and heated at 5 °C for 1 minute under an argon atmosphere. -1 The heating rate was increased to 800 °C and held at that temperature for 1 h. After the reaction was complete, the mixture was cooled to room temperature. The resulting black substance was removed, acid-washed to remove the catalyst, washed, and dried. The resulting black substance is the porous carbon material.
[0023] The specific surface area of the porous carbon material was measured to be 1050 m². 2 g -1 The iodine value of the porous carbon material was tested and found to be 1255 mg g. -1 When this porous carbon material is used as the anode material for lithium-ion batteries, the capacity is 485 mAh g. -1 When this porous carbon material is used as an electrode material for a supercapacitor, the capacitance is 205 F g. -1 .
[0024] Example 3 This embodiment provides a method for preparing porous carbon materials, wherein the preparation method includes the following specific steps: 50 g of powdered silica catalyst is added to 20 g of waste tire oil for impregnation, followed by ultrasonication for 10 minutes. The resulting mixture is placed in a ceramic boat and then placed in a horizontal tube furnace. Under an argon atmosphere, it is heated at 5 °C for 1 minute. -1 The temperature was increased to 800°C and held at that temperature for 1 hour. After the reaction was complete, it was cooled to room temperature, and the resulting black substance was removed. The catalyst was removed by acid washing, and the substance was then washed and dried. The resulting black substance is the porous carbon material. The porous carbon material prepared in Example 2 was subjected to scanning electron microscopy (SEM) testing. Figure 3 As shown, the porous carbon material exhibits a hollow spherical structure. The specific surface area of the porous carbon material was measured to be 1320 m². 2 g -1 The iodine value of the porous carbon material was tested and found to be 1380 mg g.-1 When this porous carbon material is used as the anode material for lithium-ion batteries, the capacity is 545 mAh g. -1 When this porous carbon material is used as an electrode material for a supercapacitor, Figure 4 The graph shows the rate performance of the porous carbon electrode at 1 A g. -1 The capacitance at the current density is 224 F g. -1 . Figure 5 The cyclic voltammetry curve of the porous carbon electrode is shown at 100 mV s. -1 It exhibits a good rectangular shape at a scan rate of [missing information], indicating that it has excellent double-layer storage characteristics.
[0025] Example 4 This embodiment provides a method for preparing porous carbon materials, wherein the preparation method includes the following specific steps: 30 g of powdered silica catalyst is added to 10 g of vacuum residue for impregnation, followed by ultrasonication for 10 minutes. The resulting mixture is placed in a ceramic boat and then placed in a horizontal tube furnace, and heated at 5 °C for 1 minute under an argon atmosphere. -1 The temperature was increased to 800°C and held at that temperature for 1 hour. After the reaction was complete, the mixture was cooled to room temperature, and the resulting black substance was removed. The catalyst was removed by acid washing, and the mixture was then washed and dried. The resulting black substance was the porous carbon material. The specific surface area of the porous carbon material prepared in Example 3 was tested, and the measured specific surface area was 1250 m². 2 g -1 The iodine value of the porous carbon material was tested and found to be 1310 mg g. -1 When this porous carbon material is used as the anode material for lithium-ion batteries, the capacity is 520 mAh g. -1 When this porous carbon material is used as an electrode material for supercapacitors, at 1 A g -1 The capacitance at the current density is 212 F g -1 .
[0026] Example 5 This embodiment provides a method for preparing porous carbon materials, wherein the preparation method includes the following specific steps: 30 g of powdered copper oxide catalyst is added to 10 g of vacuum wax oil for impregnation, followed by ultrasonication for 10 minutes. The resulting mixture is placed in a ceramic boat and placed in a horizontal tube furnace, and then heated at 5 °C for 1 minute under an argon atmosphere. -1 The temperature was increased to 800 °C and held at that temperature for 1 h. After the reaction was complete, it was cooled to room temperature, and the resulting black substance was removed. The catalyst was removed by acid washing, and the substance was then washed and dried. The resulting black substance was the porous carbon material. The specific surface area of the porous carbon material prepared in Example 4 was tested, and the specific surface area was measured to be 1185 m². 2 g -1The iodine value of the porous carbon material was tested and found to be 1265 mg g. -1 When this porous carbon material is used as the anode material for lithium-ion batteries, the capacity is 524 mAh g. -1 When this porous carbon material is used as an electrode material for supercapacitors, at 1 A g -1 The capacitance at the current density is 208 F g. -1 .
[0027] Example 6 This embodiment provides a method for preparing porous carbon materials, wherein the preparation method includes the following specific steps: 50 g of powdered calcium oxide catalyst is added to 10 g of waste tire oil for impregnation, followed by ultrasonication for 10 minutes. The resulting mixture is placed in a ceramic boat and then placed in a horizontal tube furnace, and heated at 5 °C for 1 minute under an argon atmosphere. -1 The temperature was increased to 800 °C and held at that temperature for 1 h. After the reaction was complete, it was cooled to room temperature, and the resulting black substance was removed. The catalyst was removed by acid washing, and the substance was then washed and dried. The resulting black substance was the porous carbon material. The specific surface area of the porous carbon material prepared in Example 5 was measured to be 1460 m². 2 g -1 The iodine value of the porous carbon material was tested and found to be 1452 mg g. -1 When this porous carbon material is used as the anode material for lithium-ion batteries, the capacity is 589 mAh g. -1 When this porous carbon material is used as an electrode material for supercapacitors, at 1 A g -1 The capacitance at the current density is 232 F g. -1 .
[0028] Comparative Example 1 This embodiment provides a method for preparing porous carbon materials, wherein the preparation method includes the following specific steps: 50 g of powdered calcium oxide catalyst is added to 10 g of waste tire oil for impregnation, followed by ultrasonication for 10 minutes. The resulting mixture is placed in a ceramic boat and then placed in a horizontal tube furnace, and heated at 10 °C for 1 minute under an argon atmosphere. -1 The temperature was increased to 1000°C and held at that temperature for 1 hour. After the reaction was complete, the mixture was cooled to room temperature, and the resulting black substance was removed. The catalyst was removed by acid washing, and the mixture was then washed and dried. The resulting black substance was the porous carbon material. The specific surface area of the porous carbon material prepared in Comparative Example 1 was measured to be 960 m². 2 g -1 The iodine value of the porous carbon material was tested and found to be 1123 mg g. -1 When this porous carbon material is used as the anode material for lithium-ion batteries, the capacity is 475 mAh g.-1 When this porous carbon material is used as an electrode material for supercapacitors, at 1 A g -1 The capacitance at the current density is 198 F g -1 .
[0029] Comparative Example 2 This embodiment provides a method for preparing porous carbon materials, wherein the preparation method includes the following specific steps: 50 g of powdered calcium oxide catalyst is added to 10 g of waste tire oil for impregnation, followed by ultrasonication for 10 minutes. The resulting mixture is placed in a ceramic boat and then placed in a horizontal tube furnace, and heated at 10 °C for 1 minute under an argon atmosphere. -1 The temperature was increased to 650 °C and held at that temperature for 1 h. After the reaction was complete, it was cooled to room temperature, and the resulting black substance was removed. The catalyst was removed by acid washing, and the substance was then washed and dried. The resulting black substance was the porous carbon material. The specific surface area of the porous carbon material prepared in Comparative Example 1 was measured to be 860 m². 2 g -1 The iodine value of the porous carbon material was tested and found to be 852 mg g. -1 When this porous carbon material is used as the anode material for lithium-ion batteries, the capacity is 425 mAh g. -1 When this porous carbon material is used as an electrode material for supercapacitors, at 1 A g -1 The capacitance at the current density is 198 F g -1 .
Claims
1. A method for preparing porous carbon materials, characterized in that, The preparation method is as follows: the powdered catalyst is placed in a rotating bed reactor, and under an inert atmosphere, it is heated at 5°C for 5 minutes. -1 -10℃min -1 The heating rate is increased to 700℃-800℃, and the gasified heavy oil is introduced into a rotating bed reactor to allow the gasified heavy oil to come into gas-solid contact with the powdered catalyst. The reaction is carried out at atmospheric pressure and constant temperature for 20-30 minutes. After the reaction is completed, the mixture is cooled to room temperature, and the resulting black substance is taken out, acid-washed to remove the catalyst, washed, and dried to obtain porous carbon material. The heavy oil is ethylene tar; The obtained porous carbon material exhibits a regular lamellar morphology with 1-2 layers; The porous carbon material has a specific surface area of 1650 m². 2 g -1 -1700m 2 g -1 .
2. The preparation method according to claim 1, characterized in that, The weight ratio of heavy oil to powdered catalyst is 10:(5-100).
3. The preparation method according to claim 1, characterized in that, The powder catalyst includes one or more of copper oxide, aluminum oxide, calcium oxide, and ferric oxide.
4. The preparation method according to claim 1, characterized in that, The inert atmosphere includes one or a combination of nitrogen, helium and argon.
5. The porous carbon material prepared by any one of claims 1-4, characterized in that, The pore size distribution is 0.5-80 nm, and the iodine value is greater than 1350 mg g. -1 .
6. The application of the porous carbon material according to claim 5 in the preparation of purification adsorption materials, catalyst supports and electrode materials.
Citation Information
Patent Citations
High-capacitance hierarchical pore carbon material, preparation method and application thereof