A high flux anti-wetting anti-fouling anti-biofouling dense Janus membrane and a method of making the same
By dissolving dopamine, polyethyleneimine, and tris(hydroxymethyl)aminomethane in water to prepare a hydrophilic modified membrane, and constructing a dense Janus membrane through interfacial polymerization, the problems of low flux and complex preparation of existing dense Janus membranes were solved, and the anti-wetting, anti-fouling, and anti-scaling properties of high flux were improved.
Patent Information
- Application Number
- CN202410667261.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-27
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-05-27
AI Technical Summary
Existing dense Janus membranes suffer from low flux in terms of antifouling, antiwetting, and antiscaling properties, and their preparation process is complex and environmentally unfriendly.
A hydrophilic modified membrane was prepared by dissolving dopamine, polyethyleneimine, and tris(hydroxymethyl)aminomethane in water and adjusting the pH to 8.5. Then, a dense Janus membrane was constructed by impregnating the membrane with a hexane solution of pyromellitic methyl chloride and carrying out an interfacial polymerization reaction.
It achieves high-throughput anti-wetting, anti-fouling, and anti-scaling properties, while simplifying the preparation process and improving the membrane's transport efficiency and environmental friendliness.
Smart Images

Figure CN118477494B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of water treatment technology, and in particular to a high-flux, anti-wetting, anti-fouling, and anti-scaling dense Janus membrane and its preparation method. Background Technology
[0002] Water pollution and water scarcity are serious challenges facing our time, posing a significant threat to the global economy, ecological environment health, and global sustainable development strategies. Membrane distillation (MD) technology is a non-isothermal membrane separation process driven by the vapor pressure gradient between the hot feed side and the cold osmotic side. Water vaporizes on the membrane surface on the hot feed side, forming steam that passes through the membrane pores and enters the cold side for condensation and enrichment. Non-volatile pollutants are retained on the feed side, simultaneously achieving the goal of obtaining purified water and concentrated wastewater. Compared with other membrane separation processes, the MD process has unique advantages, such as theoretically 100% retention of non-volatile molecules, lower operating temperature and pressure, no osmotic pressure limitations, and the ability to utilize low-quality thermal energy (such as waste heat from production, solar energy, geothermal energy, etc.) to reduce its energy consumption, making it a highly promising water treatment technology.
[0003] Despite these advantages, membrane distillation technology faces increasingly complex treatment challenges due to the development of the water industry and the demands of ecological protection. Industrial wastewater, polluted seawater or brackish water, oily wastewater, and dye wastewater inevitably contain pollutants such as hydrophobic substances, amphiphilic substances, and scaling ions, with complex compositions and varying concentrations. Even with novel MD membranes possessing different wettability surfaces, such as superhydrophobic membranes, fully hydrophobic membranes, and conventional Janus membranes (with porous hydrophilic surfaces), it is difficult to simultaneously achieve multiple resistances (two or even three of antifouling, antiwetting, and antiscaling), limiting the application range of MD. Novel dense Janus membranes, composed of a dense hydrophilic surface layer and a hydrophobic porous base membrane, may be the ideal membrane structure to simultaneously achieve multiple resistances, potentially making MD a feasible technology for treating complex wastewater. However, while the introduction of a dense layer imparts resistance, it often leads to flux reduction due to increased mass transfer resistance and temperature polarization. Furthermore, novel dense Janus membranes capable of simultaneously resisting fouling, wetting, and scaling remain lacking. Chinese patent (CN 115382403A) discloses a method for preparing a dense Janus membrane. This membrane uses a hydrophobic nanofiber membrane as the base membrane, and sequentially constructs a superhydrophilic skin layer and two ultrathin dense layers (polyamide + polyvinyl alcohol / polyacrylic acid) on its surface to obtain a composite membrane. This membrane effectively intercepts volatile pollutants in the feed liquid and exhibits good anti-wetting properties. However, the flux of this membrane is reduced by nearly 25% compared to the original membrane. Similarly, another patent (CN 116020267A) discloses a method for preparing and applying an anti-wetting dense Janus membrane. This membrane first uses a hydrophobic microporous membrane as the base membrane, and then modifies it hydrophilically through dopamine polymerization. Secondly, a dense layer is further constructed on the modified membrane through interfacial polymerization to reduce the pore size of the composite membrane. The resulting membrane exhibits excellent anti-wetting properties in the treatment of feed brine containing surfactants; however, its anti-fouling and anti-scaling properties are not mentioned. Furthermore, in the examples, the membrane flux of different membranes decreased significantly with increasing interfacial polymerization cycles. Chinese Patent (CN 116020280A) discloses a method for preparing a hydrogel Janus membrane that simultaneously exhibits anti-wetting, anti-fouling, and anti-scaling properties. This membrane is obtained by coating a hydrogel solution prepared from polyvinyl alcohol (PVA), tannic acid (TA), and cellulose nanocrystals (CNC) onto a hydrophilically modified hydrophobic membrane surface and allowing it to air dry. The resulting membrane exhibited stable molecular weight (MD) performance during treatment with an oil-water emulsion of 3.5% sodium chloride, 0.1 g / L mineral oil, and 0.4 mM sodium dodecyl sulfate. However, hydrogel Janus membranes doped with different proportions of CNC showed varying degrees of flux attenuation, even reaching as high as 50%.
[0004] Therefore, achieving the antifouling, antiwetting, and antiscaling properties of dense Janus membranes while maintaining or even increasing membrane flux is a pressing challenge for composite membrane distillation membranes. Those skilled in the art are dedicated to developing a novel high-flux, anti-wetting, antifouling, and antiscaling dense Janus membrane using simple and effective preparation methods and exploring its applications in wastewater treatment. Summary of the Invention
[0005] In view of the above-mentioned deficiencies of the prior art, the technical problem to be solved by the present invention is that existing dense Janus membranes usually have low flux, and novel fully hydrophobic membranes, superhydrophobic membranes and Janus membranes are difficult to achieve simultaneous anti-wetting, anti-fouling and anti-fouling properties. In addition, the preparation process of existing fully hydrophobic membranes and superhydrophobic membranes is complicated and environmentally unfriendly.
[0006] To achieve the above objectives, the present invention provides a method for preparing a high-flux, anti-wetting, anti-fouling, and anti-scaling dense Janus membrane, the method comprising the following steps:
[0007] Step 1: Dissolve dopamine, polyethyleneimine, and tris(hydroxymethyl)aminomethane in water in a certain proportion, adjust the pH to 8.5, and obtain a mixed solution.
[0008] Step 2: Float a commercial porous hydrophobic PVDF microfiltration membrane on the surface of the mixed solution prepared in Step 1 for a certain period of time; Remove the treated membrane, wash the membrane surface with deionized water, and then dry it to obtain a dried hydrophilic modified membrane.
[0009] Step 3: Place the hydrophilic modified membrane obtained in Step 2 in a fixture and fix it so that its modified side is exposed; then, wet the hydrophilic modified membrane with a hexane solution of trimesoyl chloride.
[0010] Step 4: Remove excess oil phase solution from the surface of the membrane after step 3, and then pour the solution containing active monomers onto its modified side surface to allow it to undergo interfacial polymerization reaction.
[0011] Step 5: Place the membrane obtained after the reaction in step 4 in an oven for heat treatment, and then wash and dry it to obtain the target dense Janus distillation membrane.
[0012] Further, in step 1, the mass concentrations of dopamine, polyethyleneimine, and tris(hydroxymethyl)aminomethane are 0.5–4.0 g / L, 0.5–4.0 g / L, and 0.5–8.0 g / L, respectively, and the molecular weight Mw of the polyethyleneimine is 200–20000 Da.
[0013] Furthermore, the nominal pore size of the commercial porous hydrophobic PVDF microfiltration membrane in step 2 is 0.22 μm, and the commercial porous hydrophobic PVDF microfiltration membrane floats on the mixed solution for 4 hours.
[0014] Furthermore, the method for drying moisture in step 2 is to place the container in a 60°C oven for drying.
[0015] Furthermore, in step 3, the concentration of the hexane solution of pyromellitic methyl methacrylate is 0.05–1.0 wt%, and the immersion time in step 3 lasts for 60 seconds.
[0016] Furthermore, the solution containing the active monomer in step 4 is an aqueous solution of tetrahydroxymethylphosphoric acid with a mass fraction of 1-20 wt%.
[0017] Furthermore, the solution containing the active monomer in step 4 is preferably an aqueous solution of tetrahydroxymethylphosphoric acid with a mass fraction of 3-15 wt%.
[0018] Furthermore, the solution containing the active monomer in step 4 is an aqueous solution of pentapentanol with a mass fraction of 1-20 wt%.
[0019] Furthermore, in step 4, the interfacial polymerization reaction time is 600s, the ambient temperature is 10-30℃, and the relative humidity is 25-75%; in step 5, the oven temperature is 60℃, and the heat treatment time is 5min.
[0020] This invention also discloses a high-flux, anti-wetting, anti-fouling, and anti-scaling dense Janus membrane, prepared using any of the above methods. The surface of the high-flux, anti-wetting, anti-fouling, and anti-scaling dense Janus membrane is dense and free of visible micropores. The water contact angle of the high-flux, anti-wetting, anti-fouling, and anti-scaling dense Janus membrane in air is 15–30°, and the oil contact angle underwater is 140–160°.
[0021] The high-flux, anti-wetting, anti-fouling, and anti-scaling dense Janus membrane of this invention is beneficial for application in the field of wastewater treatment. While increasing membrane flux, it also has strong anti-wetting, anti-fouling, and anti-scaling effects.
[0022] Compared with the prior art, the present invention has the following beneficial technical effects:
[0023] 1. Existing novel dense Janus membranes suffer from high mass transfer resistance and severe temperature polarization, resulting in low membrane flux. This invention addresses this by constructing a finely structured, dense thin layer rich in hydrophilic groups and with low permeation resistance. This weakens the hydrogen bonding between water molecules in the hydrophilic layer, reducing the energy required for evaporation. Meanwhile, the highly permeable cross-linked network structure provides rapid transport channels for water molecules, facilitating water supply and significantly improving membrane flux. By selecting active monomers with excellent hydration properties to participate in the construction of the dense hydrophilic skin layer, the proportion of intermediate water within the skin layer is increased, further reducing the energy barrier required for evaporation. Simultaneously, the formed polymer network structure has a large free volume fraction, providing a rapid channel for liquid water replenishment.
[0024] 2. The superhydrophilic, dense structure constructed by regulating the reaction ratio of active monomers in this invention can inhibit the wetting, fouling, and scaling of the membrane by pollutants in wastewater, such as surfactants, scaling ions, and oils, through size sieving, electrostatic repulsion, and hydration layers, thereby suppressing the kinetics and thermodynamics of pollutant-induced membrane wetting, fouling, and scaling. Compared with existing superhydrophobic membranes, fully hydrophobic membranes, and conventional Janus membranes, which are still sensitive to one or two of wetting, fouling, or scaling, the dense Janus membrane of this invention can simultaneously provide strong anti-wetting, anti-fouling, and anti-scaling effects.
[0025] 3. Compared with the complex and environmentally unfriendly preparation processes of existing superhydrophobic and fully hydrophobic membranes, the membrane preparation process of this invention is simple and its structure / properties are tunable. The preparation method of this invention is relatively simple and can easily and effectively finely control the structure and properties of the hydrophilic layer (such as hydrophilicity, pore size, surface chemistry, and surface morphology) to further optimize membrane performance. Interfacial polymerization technology can achieve precise and simple control over the structure and properties of dense thin layers.
[0026] The following will further explain the concept, specific structure, and technical effects of the present invention in conjunction with the accompanying drawings, so as to fully understand the purpose, features, and effects of the present invention. Attached Figure Description
[0027] Figure 1 This is a scanning electron microscope image of the PVDF microporous hydrophobic substrate membrane of Comparative Example 1 of the present invention;
[0028] Figure 2 This is a scanning electron microscope image of the dense Janus film of Embodiment 2 of the present invention;
[0029] Figure 3 These are the contact angle test results for Comparative Examples 1-2 and Examples 1-3;
[0030] Figure 4 Membrane distillation desalination experiments of Comparative Examples 1-2 and Examples 1-3 (35 g·L⁻¹) -1 Comparison of water flux and salt rejection performance in NaCl;
[0031] Figure 5 Wetting tests (35 g·L⁻¹) of the membranes in Comparative Example 1 and Example 2 -1 Figure 1 shows the changes in water flux and osmotic conductivity over time in NaCl and 0.4 mM sodium dodecyl sulfate (SDS).
[0032] Figure 6 Contamination test of Comparative Example 1 and Example 2 (35 g·L) -1 NaCl and 2g·L -1 Plot showing the changes in water flux and permeation-side conductivity in mineral oil over time.
[0033] Figure 7 This is a graph showing the changes in water flux and permeable conductivity over time in scaling tests (20 mM CaCl2, 20 mM Na2SO4) of Comparative Example 1 and Example 2. Detailed Implementation
[0034] The following description, with reference to the accompanying drawings, illustrates several preferred embodiments of the present invention to make its technical content clearer and easier to understand. The present invention can be embodied in many different forms, and the scope of protection of the present invention is not limited to the embodiments mentioned herein.
[0035] Example 1
[0036] A method for preparing a novel, high-flux, anti-wetting, anti-fouling, and anti-fouling dense Janus membrane distillation membrane includes the following steps:
[0037] Step 1: Dissolve dopamine, polyethyleneimine (Mw = 600 Da), and tris(hydroxymethyl)aminomethane (Tris) in water to prepare a mixed solution with mass concentrations of 2.0 g / L, 2.0 g / L, and 1.0 g / L for dopamine, polyethyleneimine, and tris(hydroxymethyl)aminomethane (Tris), and adjust the pH to 8.5.
[0038] Step 2: Float a commercial porous hydrophobic PVDF microfiltration membrane (model: GVHP04700; nominal pore size: 0.22 μm) on the surface of the above mixed solution for 4 hours. Remove the treated membrane, wash the membrane surface with deionized water, and then place it in a 60°C oven to dry the moisture, obtaining a dried hydrophilic modified membrane.
[0039] Step 3: Place the modified PVDF microfiltration membrane from Step 2 in a fixture and fix it in place, exposing only the modified side. Wet the membrane with a hexane solution containing 0.2 wt% trimesoyl chloride (TMC) for 60 seconds.
[0040] Step 4: Remove excess oil phase solution from the membrane surface from Step 3, then directly pour a 3 wt% aqueous solution of tetramethylolphosphine chloride (THPC) onto its modified side surface to initiate interfacial polymerization. This process lasts 600 s. The ambient temperature is 20°C and the relative humidity is 50%.
[0041] Step 5: Place the membrane obtained after the reaction in step 4 in an oven at 60°C for 5 minutes for heat treatment, and then wash and dry to obtain the target dense Janus membrane.
[0042] Example 2
[0043] A method for preparing a novel high-flux, wettable, fouling-resistant, and scale-resistant dense Janus membrane distillation membrane is disclosed. The only difference between this method and Example 1 is that the concentration of tetrahydroxymethyl phosphorus chloride (THPC) aqueous solution used in step 4 is 15 wt%. All other conditions, parameters, and steps are the same as in Example 1.
[0044] Example 3
[0045] A method for preparing a novel high-flux, wettable, fouling-resistant, and scale-resistant dense Janus membrane distillation membrane is disclosed. The difference between this method and Example 2 is that the active monomer used in step 4 is changed from tetrahydroxymethylphosphoric chloride (THPC) to pentapentanol at a concentration of 15 wt%. All other conditions, parameters, and steps are the same as in Example 2.
[0046] Example 4
[0047] A method for preparing a novel high-flux, wettable, fouling-resistant, and scale-resistant dense Janus membrane distillation membrane is disclosed. The difference between this method and Example 2 is that the active monomer used in step 4 is changed from tetrahydroxymethylphosphoric chloride (THPC) to pentapentanol at a concentration of 20 wt%. All other conditions, parameters, and steps are the same as in Example 2.
[0048] Example 5
[0049] A method for preparing a novel, high-flux, anti-wetting, anti-fouling, and anti-fouling dense Janus membrane distillation membrane includes the following steps:
[0050] Step 1: Dissolve dopamine, polyethyleneimine (Mw = 200 Da), and tris(hydroxymethyl)aminomethane (Tris) in water to prepare a mixed solution with mass concentrations of 0.5 g / L, 0.5 g / L, and 0.5 g / L of dopamine, polyethyleneimine, and tris(hydroxymethyl)aminomethane (Tris), and adjust the pH to 8.5.
[0051] Step 2: Float a commercial porous hydrophobic PVDF microfiltration membrane (model: GVHP04700; nominal pore size: 0.22 μm) on the surface of the above mixed solution for 4 hours. Remove the treated membrane, wash the membrane surface with deionized water, and then place it in a 60°C oven to dry the moisture, obtaining a dried hydrophilic modified membrane.
[0052] Step 3: Place the modified PVDF microfiltration membrane from Step 2 in a fixture and fix it in place, exposing only the modified side. Wet the membrane with a hexane solution containing 0.05 wt% trimesoyl chloride (TMC) for 60 seconds.
[0053] Step 4: Remove excess oil phase solution from the membrane surface from Step 3, then directly pour a 1 wt% aqueous solution of tetramethylolphosphine chloride (THPC) onto its modified side surface to induce interfacial polymerization. This process lasts 600 s. The ambient temperature is 10°C and the relative humidity is 25%.
[0054] Step 5: Place the membrane obtained after the reaction in step 4 in an oven at 60°C for 5 minutes for heat treatment, and then wash and dry to obtain the target dense Janus membrane.
[0055] Example 6
[0056] A method for preparing a novel, high-flux, anti-wetting, anti-fouling, and anti-fouling dense Janus membrane distillation membrane includes the following steps:
[0057] Step 1: Dissolve dopamine, polyethyleneimine (Mw = 20000 Da), and tris(hydroxymethyl)aminomethane (Tris) in water to prepare a mixed solution with mass concentrations of 4.0 g / L, 4.0 g / L, and 8.0 g / L for dopamine, polyethyleneimine, and tris(hydroxymethyl)aminomethane (Tris), and adjust the pH to 8.5.
[0058] Step 2: Float a commercial porous hydrophobic PVDF microfiltration membrane (model: GVHP04700; nominal pore size: 0.22 μm) on the surface of the above mixed solution for 4 hours. Remove the treated membrane, wash the membrane surface with deionized water, and then place it in a 60°C oven to dry the moisture, obtaining a dried hydrophilic modified membrane.
[0059] Step 3: Place the modified PVDF microfiltration membrane from Step 2 in a fixture and fix it in place, exposing only the modified side. Wet the membrane with a hexane solution containing 1.0 wt% trimesoyl chloride (TMC) for 60 seconds.
[0060] Step 4: Remove excess oil phase solution from the membrane surface from Step 3, then directly pour a 20 wt% aqueous solution of tetramethylolphosphine chloride (THPC) onto its modified side surface to initiate interfacial polymerization. This process lasts 600 s. The ambient temperature is 30°C and the relative humidity is 75%.
[0061] Step 5: Place the membrane obtained after the reaction in step 4 in an oven at 60°C for 5 minutes for heat treatment, and then wash and dry to obtain the target dense Janus membrane.
[0062] Comparative Example 1
[0063] A PVDF porous hydrophobic base membrane with a diameter of 5 cm, model number GVHP04700, was purchased from Millipore.
[0064] Comparative Example 2
[0065] A method for preparing a dense Janus membrane, steps 1 and 2 are the same as in Example 1.
[0066] Step 3: Place the modified PVDF microfiltration membrane from Step 2 in a fixture and fix it in place, exposing only the modified side. Wet the membrane with a 1 wt% PIP solution, and then remove excess solution from the surface.
[0067] Step 4: Pour a 0.2 wt% solution of trimesoyl chloride (TMC) in hexane onto the surface to initiate interfacial polymerization. This process lasts 120 seconds. The ambient temperature is approximately 20°C, and the relative humidity is approximately 50%.
[0068] Step 5: The hydrophilic surface of the membrane obtained after the reaction in Step 4 is washed several times with hexane / deionized water to remove unreacted active monomers. The membrane is then heat-treated in an oven at 60°C for 5 minutes to obtain the target dense Janus membrane.
[0069] (1) Morphological comparison
[0070] The surface morphology of Comparative Example 1 and Example 2 was characterized using scanning electron microscopy. Figure 1 The morphology of the PVDF microporous hydrophobic base membrane in Comparative Example 1 shows a typical porous structure. Figure 2 The dense Janus film obtained by hydrophilic modification of the hydrophobic base film surface and subsequent interfacial polymerization reaction in Example 2 exhibits a granular and dense surface with no visible micropores.
[0071] (2) Contact angle test
[0072] The contact angles of water in air and oil (mineral oil) underwater were tested using a Dropmeter A-200 contact angle meter from MAIST Corporation, China. Comparative Examples 1-2 and Examples 1-3 were measured respectively. The volume of both water and oil droplets was 9 μL. Figure 3 As shown, compared to the hydrophobic surface of Comparative Example 1, Comparative Example 2 and Examples 1-3 all successfully constructed hydrophilic surfaces. Among them, the water contact angle of Example 2 is only about 20°, which is significantly enhanced in hydrophilicity compared to other membranes. At the same time, Example 2 exhibits strong underwater superoleophobic properties, with an underwater contact angle of 154.2°.
[0073] (3) Membrane distillation (MD) test
[0074] The dense Janus membranes prepared in Comparative Examples 1-2 and Examples 1-3 were used for MD testing, and were used to treat samples containing 35 g·L⁻¹ of organic matter. -1 The performance of NaCl salt solutions was compared. Subsequently, the dense Janus membrane prepared in Example 2 was used for wetting (35 g·L⁻¹). -1 NaCl and 0.4 mM sodium dodecyl sulfate (SDS)), pollution (35 g·L) -1 NaCl and 2g·L -1 Mineral oil) and scaling experiments (20 mM CaCl2, 20 mM Na2SO4) were conducted and compared with Comparative Example 1. Membrane distillation parameters were set as follows: feed side temperature 60℃, permeate side temperature 20℃, and flow rate 0.5 LPM. The mass of the permeate side solution was recorded using an electronic balance, and the conductivity of the distillation side water was monitored using a conductivity meter. Salt rejection rate (SR) = 1 - permeate side salt concentration (C p ) / Feed-side salt concentration (C f Since salt concentration is directly proportional to conductivity at a given temperature, the ratio of permeation-side conductivity to feed-side conductivity can be approximated as the salt concentration ratio. The test results are as follows... Figures 4-7 As shown.
[0075] according to Figure 4 It can be seen that the novel dense Janus membrane provided by this invention has a significantly improved membrane flux. Specifically, the novel dense Janus membrane prepared in Example 2 was treated at 60°C for 35 g·L⁻¹. -1 The membrane flux of the NaCl brine solution was approximately 34 LMH. The novel dense Janus membrane prepared in Example 2 showed an approximately 20% increase in flux compared to Comparative Example 1, and a significant 40% increase compared to Comparative Example 2. All membranes maintained 100% salt rejection during desalination.
[0076] according to Figure 5It can be seen that the novel dense Janus membrane provided by this invention also possesses high anti-wetting properties. Specifically, the novel dense Janus membrane prepared in Example 2 can efficiently and stably treat saline wastewater containing 0.4 mM surfactant SDS. In contrast, Comparative Example 1 membrane failure occurred rapidly (<15 min), losing its water vapor mass transfer and salt interception performance (the permeate-side conductivity increased significantly, indicating salt leakage).
[0077] according to Figure 6 It can be seen that the novel dense Janus membrane provided by this invention also exhibits high fouling capacity. Specifically, the novel dense Janus membrane prepared in Example 2, when treating a concentration of 2 g·L⁻¹, demonstrates good performance. -1 When exposed to high-salinity wastewater containing mineral oil, its molecular weight distribution (MD) performance remained stable. In contrast, Comparative Example 1 gradually lost its flux within 2.5 hours.
[0078] according to Figure 7 It can be seen that the novel dense Janus membrane provided by this invention also possesses high anti-fouling properties. Specifically, the novel dense Janus membrane prepared in Example 2 maintained stable MD performance during a 10-hour test period when treating brine containing 20 mM CaCl2 and 20 mM Na2SO4. In contrast, Comparative Example 1 showed a gradual decrease in flux during the 10-hour operation, accompanied by a significant increase in permeate-side conductivity.
[0079] The preferred embodiments of the present invention have been described in detail above. It should be understood that those skilled in the art can make numerous modifications and variations based on the concept of the present invention without creative effort. Therefore, all technical solutions that can be obtained by those skilled in the art based on the concept of the present invention through logical analysis, reasoning, or limited experimentation on the basis of existing technology should be within the scope of protection defined by the claims.
Claims
1. A method for preparing a high-flux, anti-wetting, anti-fouling, and anti-scaling dense Janus membrane, characterized in that, The method includes the following steps: Step 1: Dissolve dopamine, polyethyleneimine, and tris(hydroxymethyl)aminomethane in water in a certain proportion, adjust the pH to 8.5, and obtain a mixed solution. Step 2: Float a commercial porous hydrophobic PVDF microfiltration membrane on the surface of the mixed solution prepared in Step 1 for a certain period of time; Remove the treated membrane, wash the membrane surface with deionized water, and then dry it to obtain a dried hydrophilic modified membrane. Step 3: Place the hydrophilic modified membrane obtained in Step 2 in a fixture and fix it so that its modified side is exposed; then, wet the hydrophilic modified membrane with a hexane solution of trimesoyl chloride. Step 4: Remove excess oil phase solution from the surface of the membrane after step 3 treatment, and then pour the solution containing active monomers onto its modified side surface to allow it to undergo interfacial polymerization reaction; the solution containing active monomers in step 4 is an aqueous solution of tetramethylphosphoric acid with a mass fraction of 1~20wt% or an aqueous solution of pentapentanol with a mass fraction of 1~20wt%. Step 5: Place the membrane obtained after the reaction in step 4 in an oven for heat treatment, and then wash and dry it to obtain the target dense Janus membrane.
2. The method for preparing a high-flux, anti-wetting, anti-fouling, and anti-scaling dense Janus membrane as described in claim 1, characterized in that, In step 1, the mass concentrations of dopamine, polyethyleneimine, and tris(hydroxymethyl)aminomethane are 0.5~4.0 g / L, 0.5~4.0 g / L, and 0.5~8.0 g / L, respectively, and the molecular weight Mw of the polyethyleneimine is 200~20000 Da.
3. The method for preparing a high-flux, anti-wetting, anti-fouling, and anti-scaling dense Janus membrane as described in claim 1, characterized in that, The nominal pore size of the commercial porous hydrophobic PVDF microfiltration membrane in step 2 is 0.22 μm, and the commercial porous hydrophobic PVDF microfiltration membrane floats on the mixed solution for 4 hours.
4. The method for preparing a high-flux, anti-wetting, anti-fouling, and anti-scaling dense Janus membrane as described in claim 1, characterized in that, The method for drying moisture in step 2 is to place the container in a 60°C oven for drying.
5. The method for preparing a high-flux, anti-wetting, anti-fouling, and anti-scaling dense Janus membrane as described in claim 1, characterized in that, In step 3, the concentration of the hexane solution of pyromellitic methyl methacrylate chloride is 0.05~1.0wt%, and the immersion time in step 3 lasts for 60s.
6. The method for preparing a high-flux, anti-wetting, anti-fouling, and anti-scaling dense Janus membrane as described in claim 1, characterized in that, The interfacial polymerization reaction time in step 4 is 600s, the ambient temperature is 10~30℃, and the relative humidity is 25~75%; the oven temperature in step 5 is 60℃, and the heat treatment time is 5min.
7. A high-flux, anti-wetting, anti-fouling, and anti-scaling dense Janus membrane, characterized in that, The high-flux, anti-wetting, anti-fouling, and anti-scaling dense Janus membrane, prepared using any one of claims 1 to 6, has a dense surface without visible micropores, and exhibits a water contact angle of 15-30° in air. o The underwater oil contact angle is 140~160 degrees. o .
Citation Information
Patent Citations
Composite membrane with volatile substance interception characteristic for membrane distillation and preparation method of composite membrane
CN115382403A
Thin-layer composite membrane for anti-wetting membrane distillation as well as preparation method and application of thin-layer composite membrane
CN116020267A
Preparation method of hydrogel Janus membrane with wetting resistance, pollution resistance and scaling resistance
CN116020280A
Non-pressure driven nanofiltration separation membrane, preparation method and application
CN113457462A
Method for preparing anti-pollution composite nanofiltration membrane from alcohol compound
CN114307677A