A c3 fraction selective hydrogenation catalyst, its preparation method and application
By combining graphene-coated nanodiamond composite support with Pd co-active metal components, the problem of unstable performance of existing C3 fraction selective hydrogenation catalysts was solved, achieving highly active and selective conversion of propyne and propadiene into propylene, and simplifying the catalyst preparation process.
Patent Information
- Application Number
- CN202310118456.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-13
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2043-02-13
AI Technical Summary
Existing C3 fraction selective hydrogenation catalysts have complex production processes, unstable performance, and are difficult to meet the requirements of industrial applications.
Graphene-coated nanodiamonds were used as a composite support, combined with Pd and co-active metal components Cu, Au, As, Sn, and Pb. The catalyst was loaded by impregnation or deposition precipitation methods to optimize the interaction between the support and the metal and enhance the adsorption capacity of propyne and propadiene.
This improved the activity and selectivity of the catalyst, simplified the preparation process, and resulted in a catalyst product with stable performance.
Smart Images

Figure BDA0004083081710000071 
Figure BDA0004083081710000081 
Figure BDA0004083081710000091
Abstract
Description
Technical Field
[0001] This invention belongs to the field of catalyst technology, specifically relating to a selective hydrogenation catalyst for C3 fractions, its preparation method, and its application. Background Technology
[0002] In units that produce ethylene and propylene from light hydrocarbon steam cracking, the C3 fraction obtained through distillation typically contains 2%–5% propyne and propadiene. Propylene and propadiene are impurities in the propylene product, which can reduce catalyst activity during propylene polymerization, increase catalyst consumption in polypropylene, and degrade the performance of the polypropylene product. Generally, hydrogenation is used to convert propyne and propadiene into propylene, thus removing the impurities and increasing the propylene yield.
[0003] Industrial C3 fraction selective hydrogenation catalysts are prepared using palladium as the main active component and alumina as the support via an equal-volume impregnation method. To improve the hydrogenation activity and selectivity of the catalyst, the palladium loading method can be optimized, a second metal promoter such as Ag or Pb can be added, and the preparation method of the alumina support can be improved. Among these, the alumina support has a significant impact on catalyst performance. By optimizing the alumina support molding method, adding modifying agents, and preparing composite supports based on alumina, the physical pore structure and surface chemisorption properties of the alumina support can be improved, thereby enhancing the hydrogenation performance of the catalyst.
[0004] Chinese patent CN1279126A discloses a catalyst using diatomaceous earth, SiO2, TiO2, Al2O3, etc. as supports, and loaded with metal components such as Pd and Bi. This catalyst exhibits high selectivity and high activity in selective hydrogenation reactions, while reducing the amount of green oil generated and extending the catalyst life.
[0005] Chinese patent CN1958155A discloses an alkyne selective hydrogenation catalyst that uses Pd as the main active component and Ag, alkali metals, etc. as co-active components, to coat an Al2O3 coating on a talc, refractory clay, or silicon carbide inert support. By controlling the thickness of the alumina coating, the distribution of the metal active components on the support surface can be promoted, thereby improving the hydrogenation performance.
[0006] Chinese patent CN109174085A discloses a catalyst for obtaining atomically dispersed palladium nanoparticles on a diamond / graphene composite material and its preparation method. At a reaction temperature of 180℃, the selectivity of alkyne hydrogenation to olefins can reach 90%, showing high selectivity. However, the catalyst has low activity, and the alkyne conversion rate exceeds 20% at temperatures above 100℃, which cannot meet the requirements for industrial applications.
[0007] Existing C3 hydrogenation catalysts and their corresponding preparation methods suffer from problems such as long production processes, complex preparation methods, and significant performance differences between different batches of catalysts. Therefore, there is a need to develop a C3 selective hydrogenation catalyst with a simple preparation process, stable performance, and good activity and selectivity. Summary of the Invention
[0008] To address the technical problems existing in the prior art, this invention provides a novel C3 selective hydrogenation catalyst for the selective hydrogenation of propyne and propadiene in C3 fractions to produce propylene.
[0009] One objective of this invention is to provide a C3 fraction selective hydrogenation catalyst, comprising a main active metal component, an optional co-active metal component, and a composite support, wherein the main active metal component is Pd, the co-active metal component is selected from at least one of Cu, Au, As, Sn, Cr, and Pb, and the composite support comprises at least one of inorganic oxides, diatomaceous earth, molecular sieves, and graphene-coated nanodiamonds.
[0010] According to an embodiment of the present invention, the inorganic oxide is selected from at least one of Al2O3, SiO2, TiO2, and MgO. The shape of the additive is not particularly limited and can be spherical, cylindrical, toothed, strip-shaped, clover-shaped, or four-leaf clover-shaped, preferably spherical, cylindrical, or toothed, or other shapes with a regular appearance.
[0011] According to an embodiment of the present invention, the number of graphene layers in the graphene-coated nanodiamond is 1 to 3.
[0012] According to embodiments of the present invention, the content of the main active metal component in the catalyst, by mass percentage, is 0.01-2%, for example, any value or range between any two values from 0.01%, 0.05%, 0.1%, 0.5%, 1.0%, 1.5%, to 2%. Preferably, the content of the main active metal component is 0.01-1.5%, more preferably 0.05-1%. The content of the auxiliary active metal component is 0-20%, for example, 0%, 0.01%, 0.1%, 0.5%, 1%, to 2%. The content of the auxiliary active metal component is preferably 0-10%, more preferably 0-5%, and can be any value or any range between two values from 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40% to 5% by mass percentage. The content of the graphene-coated nanodiamond carrier in the composite carrier is 5-40%, for example, any value or any range between two values from 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%. Preferably, the content of the graphene-coated nanodiamond carrier is 5-20%.
[0013] According to an embodiment of the present invention, in the catalyst, the particle size of Pd is 0.1–10 nm, preferably 0.2–5 nm; the main metal active component palladium is attached to the support in the form of nanoparticles. Before evaluating the catalyst, hydrogen reduction is performed to obtain palladium and auxiliary metal nanoparticles loaded on the support. The hydrogen reduction process can employ commonly used techniques in the art.
[0014] According to an embodiment of the present invention, the specific surface area of the composite carrier is 1 to 400 m². 2 / g, bulk density is 0.3~1.5ml / g, and water absorption rate is 20~100%.
[0015] According to an embodiment of the present invention, the composite carrier further contains an adhesive, preferably selected from at least one of hydroxymethyl cellulose, polyvinyl alcohol, and starch; the content of the adhesive is 1-30% based on 100% of the total weight of the composite carrier.
[0016] A second objective of this invention is to provide a method for preparing the above-mentioned catalyst, comprising: loading the main active metal component and an optional co-active metal component onto a composite support to obtain the C3 fraction selective hydrogenation catalyst.
[0017] According to an embodiment of the present invention, the preparation method specifically includes:
[0018] Method 1: Impregnate the composite support in a metal compound solution containing the main active metal component and an optional co-active metal component, and dry to obtain the C3 fraction selective hydrogenation catalyst; or,
[0019] Method 2: A metal compound solution containing the main active metal component and an optional auxiliary active metal component is added dropwise to a composite support dispersion, heated and stirred, cooled, washed, and dried to obtain the C3 fraction selective hydrogenation catalyst.
[0020] According to embodiments of the present invention, the metal compound is selected from at least one of the following: chloride, nitrate, acetate, sulfate, oxide, and organometallic compounds of an active metal and an optional co-active metal; preferably, at least one of the following: chloride, nitrate, and acetate of an active metal and an optional co-active metal; the solvent of the metal compound solution is selected from at least one of water, hydrochloric acid, nitric acid, acetic acid, and alcohol; preferably, water; the content of the metal compound in the metal compound solution is 0.01–500 mg / mL, for example, it can be any value or a range between any two values from 0.01, 1, 10, 50, 100, 150, 200, 250, 300, 350, 400, 450, 500 mg / mL.
[0021] According to an embodiment of the present invention, the catalyst impregnated with the metal active component should be thoroughly dried. Drying can be carried out in air or under vacuum, preferably in air. Specifically, the drying conditions are: a drying temperature of 50–200°C, preferably 50–100°C; and a drying time of 5–48 h, preferably 5–24 h.
[0022] According to an embodiment of the present invention, in method two, the pH value of the composite carrier dispersion is greater than 9. The pH value of the solution can be adjusted using a commonly used alkaline compound or its solution, such as at least one of sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, potassium hydroxide, sodium hydroxide, or their aqueous solutions. In method two, the heating and stirring conditions are: stirring at 60–120°C for 0.5–10 hours.
[0023] According to an embodiment of the present invention, the composite carrier is prepared by the following method: a component comprising at least one of inorganic oxides, diatomaceous earth, molecular sieves, and graphene-coated nanodiamonds is added to a binder and mixed to form a composite. The binder is selected from at least one of hydroxymethyl cellulose, polyvinyl alcohol, and starch; the content of the binder is 1-30% based on 100% of the total weight of the composite carrier.
[0024] According to an embodiment of the present invention, the graphene-coated nanodiamond is obtained by calcining nanodiamond. Preferably, the calcination conditions are: calcination temperature of 900–1200°C and calcination time of 3–6 hours in a protective atmosphere. Specifically, the following operation can be adopted: placing the nanodiamond in a tube furnace and calcining it at an inert atmosphere (such as nitrogen) and 900–1200°C for 3–6 hours can obtain graphene-coated nanodiamond with 1–3 graphene layers.
[0025] The present invention can use common loading methods to load the metal active component precursor compound onto the support, for example, the impregnation method or the deposition precipitation method can be used to load it onto the support.
[0026] When using the impregnation method, either equal-volume impregnation or supersaturated impregnation can be employed. When using the supersaturated impregnation method, if the active component precursor in the impregnation solution cannot be completely adsorbed by the composite support, the volume of the impregnation solution and the concentration of the active component should be determined based on the adsorption ratio to ensure that the content of the active component loaded onto the composite support meets the predetermined requirements. One-step impregnation or stepwise impregnation can also be used. In the one-step impregnation method, the Pd solution and the auxiliary agent solution are mixed, and the composite support is impregnated according to the required total solution volume. For active component precursors that cannot be prepared into the same solution, a stepwise impregnation method can be used. Several active component precursors are prepared separately into solutions for impregnation of the composite support. After each impregnation, appropriate drying is performed before impregnating with another component precursor solution.
[0027] When using the deposition-precipitation method, loading should be carried out in an alkaline environment with a solution pH greater than 9 and a deposition temperature of 60–120°C. Those skilled in the art can determine the deposition reaction parameters based on the content of the active metal component in the catalyst. The solution pH can be adjusted using commonly used alkaline compounds or solutions thereof, such as at least one of sodium carbonate, sodium bicarbonate, potassium carbonate, potassium bicarbonate, potassium hydroxide, sodium hydroxide, or their aqueous solutions. Specifically, the operation can be as follows: after preheating the alkaline (pH greater than 9) composite support dispersion, the metal compound solution is slowly added dropwise to the preheated composite support dispersion under stirring. After the addition is complete, heating and stirring continue, followed by cooling to room temperature. The solid components are washed with deionized water, dried, and calcined to obtain the C3 fraction selective hydrogenation catalyst.
[0028] The third objective of this invention is to provide the above-mentioned selective hydrogenation catalyst for C3 fractions, or the selective hydrogenation catalyst for C3 fractions obtained by the above preparation method, for the application of selective hydrogenation of propyne and propadiene in C3 fractions to produce propylene.
[0029] The C3 selective hydrogenation catalyst and its preparation method of the present invention have the following advantages:
[0030] (1) The C3 selective hydrogenation catalyst provided by the present invention has better activity and selectivity because the graphene-encapsulated nanodiamonds in the support optimize the interaction between the support and the metal active components, enhance the adsorption capacity of propyne and propadiene, and weaken the adsorption of propylene.
[0031] (2) In the preparation process of the composite carrier of the present invention, the addition of the adhesive promotes the combination of graphene nanodiamond and inorganic oxide, and increases the porosity of the carrier.
[0032] (3) By controlling the structure and doping amount of graphene-encapsulated nanodiamonds during the preparation process of the catalyst of the present invention, the hydrogenation performance of the catalyst can be effectively adjusted, simplifying the control parameters in the catalyst preparation process and facilitating the obtaining of a catalyst product with stable performance. Detailed Implementation
[0033] The present invention will now be described in detail with reference to specific embodiments. It should be noted that the following embodiments are only used to further illustrate the present invention and should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the content of the present invention are still within the scope of protection of the present invention.
[0034] Unless otherwise specified, the raw materials used in the examples and comparative examples are all disclosed in the prior art, such as those that can be directly purchased or prepared according to the preparation methods disclosed in the prior art.
[0035] Preparation Example 1
[0036] Preparation method of graphene-coated nanodiamonds:
[0037] Nanodiamonds prepared by detonation were calcined under nitrogen at a temperature of 1200°C for 5 hours to obtain graphene-coated nanodiamonds. The graphene-coated nanodiamonds prepared by the above method have a core-shell structure with graphene as the shell and nanodiamond as the core; in the core-shell structure, the number of graphene shell layers is 1 to 3.
[0038] Preparation Example 2
[0039] Preparation method of composite carrier:
[0040] The composite carrier is prepared by thoroughly mixing graphene-coated nanodiamonds, at least one of inorganic oxides, diatomaceous earth, and molecular sieves with a binder, and then granulating and molding the mixture. The specific composition and amount of the composite carrier are shown in Tables 1 and 2.
[0041] The composite carrier prepared in the above manner has a specific surface area of 250–350 m². 2 / g, bulk density is 0.3~0.7ml / g, and water absorption rate is 20~75%.
[0042] Example 1
[0043] 1000 mL of deionized water was added to a flask, and the pH was adjusted to 10 with 0.1 mol / L Na₂CO₃ solution. 100 g of support (graphene-coated nanodiamond (18 wt%) + Al₂O₃ (82 wt%)) was weighed and added to the above solution, and preheated in an oil bath at 100 °C. Based on the Pd loading, a 1 mg / mL Pd(NO₃)₂ solution was taken, and the pH was adjusted to neutral by adding 0.1 mol / L Na₂CO₃ solution dropwise. The Pd solution was slowly added dropwise to the solution containing the support, and stirred for 2 hours in an oil bath at 100 °C. The resulting mixed solution was cooled to room temperature, filtered, and washed three times with deionized water. The obtained catalyst was dried in an oven at 80 °C for 10 hours to obtain catalyst A with a Pd content of 0.1%. After hydrogen reduction, the Pd particle size in catalyst A was measured to be 0.5–3 nm.
[0044] Examples 2-4
[0045] Following the method of Example 1, except that the components mixed with the graphene-coated nanodiamonds were different, catalysts B to D were prepared in Examples 2 to 4, each with a Pd content of 0.1%. After hydrogen reduction, the particle size of Pd in catalysts B to D was measured to be 0.5–5 nm. Specifically, SiO2 was used in Example 2, H-ZSM-5 was used in Example 3, and TiO2 was used in Example 4.
[0046] Table 1. Components and dosages in the composite carrier
[0047]
[0048] Example 5
[0049] 100g of support (graphene-coated nanodiamond (18wt%) + Al2O3 (82wt%)) was weighed; according to the Pd loading, a 1mg / mL Pd(NO3)2 solution was diluted with deionized water to 80mL; the support was immersed in the Pd-containing solution and impregnated at 40℃ for 5hr. Then, 50mL of C2H5OH was added, and the solvent was removed by vacuum evaporation in a rotary evaporator. The resulting catalyst was dried in an oven at 80℃ for 12hr and labeled as catalyst E, with a Pd content of 0.08%. After hydrogen reduction, the Pd particle size in catalyst E was measured to be 1–4nm.
[0050] Examples 6-8
[0051] Following the method of Example 5, the differences were that the Pd content was different and different auxiliary metal components were added to the impregnation solution. In Example 6, a certain amount of silver nitrate was added to the metal compound solution; in Example 7, a certain amount of copper nitrate was added to the metal compound solution; and in Example 8, a certain amount of stannous chloride solution was added to the metal compound solution. Catalysts F to H were obtained from Examples 6 to 8, respectively. After hydrogen reduction, the particle size of Pd in catalysts F to H was measured to be 1 to 5 nm.
[0052] Table 2. Catalyst components obtained in Examples 5-8
[0053]
[0054] Comparative Example 1
[0055] A Pd / Al₂O₃ catalyst with Ag additive was prepared by supersaturated impregnation. 20 mL of a 10 mg Pd / mL palladium nitrate solution was diluted to 80 mL with deionized water, and 0.236 g of silver nitrate was added. The solution was then impregnated onto 100 g of spherical Al₂O₃ support, dried at 120 °C for 12 hours, and calcined at 600 °C with air for 4 hours to obtain the catalyst with a Pd content of 0.2% and an Ag content of 0.15%.
[0056] Comparative Example 2
[0057] The preparation method is the same as in Example 1. In Comparative Example 2, the composite carrier in Example 1 is replaced with an equal mass of graphene-coated nanodiamond carrier.
[0058] Comparative Example 3
[0059] The preparation method was the same as in Example 1, but no adhesive was added when preparing the composite carrier in Comparative Example 3.
[0060] Test case
[0061] The above catalyst was used in a selective hydrogenation experiment of C3 fraction propyne and propadiene, under the following reaction conditions:
[0062] 50 ml of catalyst was loaded into a stainless steel tube reactor. After purging with nitrogen, hydrogen was introduced and the reactor was activated at 90°C for 2 hours. The reactor was then cooled to room temperature, purged with nitrogen, and the reactants were mixed with hydrogen and introduced into the reactor. The composition (molar fraction) of the reactants was: propane 4.99%, propylene 92.3%, propadiene 1.19%, and propyne 1.39%. The molar ratio of hydrogen to alkynes (propyne and propadiene) was 1.0–1.2, and the reaction space velocity was 100 hr. -1 The reactor inlet temperature is 33℃ and the reaction pressure is 2.0MPa.
[0063] The selective hydrogenation performance of the above catalysts for propyne and propadiene was evaluated. The conversion rates and corresponding selectivities of propyne and propadiene to propylene under the same reaction conditions are listed in Table 3 below. The conversion rate (%) and selectivity (%) of propyne and propadiene (collectively referred to as MAPD in the table) were calculated as follows:
[0064]
[0065]
[0066] Table 3. Evaluation results of catalysts obtained in the examples and comparative examples
[0067] catalyst MAPD conversion rate (%) Selectivity (%) Example 1 A 75.4 85.0 Example 2 B 72.7 81.9 Example 3 C 70.5 79.8 Example 4 D 72.1 86.3 Example 5 E 74.1 80.3 Example 6 F 81.8 96.2 Example 7 G 82.4 95.3 Example 8 H 78.0 90.2 Comparative Example 1 69.1 79.4 Comparative Example 2 21.3 95.4 Comparative Example 3 69.3 81.1
[0068] Experimental results show that the catalyst of the present invention exhibits higher activity and selectivity than the comparative example when used for the selective hydrogenation reaction of propyne and propadiene.
Claims
1. A selective hydrogenation catalyst for C3 fractions, comprising a main active metal component, a co-active metal component, and a composite support, wherein, The primary active metal component is Pd, and the secondary active metal component is selected from at least one of Cu, Au, As, Sn, Cr, and Pb. The composite support includes at least one of inorganic oxides, diatomaceous earth, and molecular sieves, and graphene-coated nanodiamonds. The inorganic oxide is selected from at least one of Al2O3, SiO2, TiO2, and MgO. In the catalyst, the particle size of Pd is 0.1~10 nm. By mass percentage, the content of the primary active metal component in the catalyst is 0.01~2%, and the content of the secondary active metal component is 0~20% but not 0. By mass percentage, the content of the graphene-coated nanodiamond support in the composite support is 5~40%.
2. The catalyst according to claim 1, characterized in that, The graphene-coated nanodiamond has 1 to 3 layers of graphene.
3. The catalyst according to claim 1, characterized in that, In the catalyst, the Pd particle size is 0.2~5 nm; and / or, The specific surface area of the composite carrier is 1~400 m². 2 / g, water absorption rate 20~100%; and / or, The composite carrier also contains an adhesive.
4. The catalyst according to claim 3, characterized in that, The catalyst, by mass percentage, contains 0.01–1.5% of the main active metal component; and / or, In terms of mass percentage, the catalyst contains 0-10% but not 0% of the co-active metal component; and / or, In terms of mass percentage, the graphene-coated nanodiamond carrier in the composite carrier comprises 5-20%; and / or, In the catalyst, the Pd particle size is 0.2~5 nm; and / or, The adhesive is selected from at least one of hydroxymethyl cellulose, polyvinyl alcohol, and starch; the content of the adhesive is 1-30% based on the total weight of the composite carrier (100%).
5. A method for preparing the catalyst according to any one of claims 1 to 4, comprising: By loading the main active metal component and the co-active metal component onto a composite support, the C3 fraction selective hydrogenation catalyst is obtained.
6. The preparation method according to claim 5, characterized in that, The preparation method specifically includes: Method 1: Impregnate the composite support in a metal compound solution containing the main active metal component and the co-active metal component, and dry to obtain the C3 fraction selective hydrogenation catalyst; or, Method 2: A metal compound solution containing the main active metal component and the auxiliary active metal component is added dropwise to a composite support dispersion, heated and stirred, cooled, washed, and dried to obtain the C3 fraction selective hydrogenation catalyst.
7. The preparation method according to claim 6, characterized in that, The metal compound is selected from at least one of the following: chlorides, nitrates, acetates, sulfates, oxides, and organometallic compounds of the primary and secondary active metals; and / or, The solvent in the metal compound solution is selected from at least one of water, hydrochloric acid, nitric acid, acetic acid, and alcohol; and / or, The metal compound solution contains 0.01~500 mg / mL of the metal compound; and / or, The drying conditions are: drying temperature of 50~200℃ and drying time of 5~48h.
8. The preparation method according to claim 7, characterized in that, The metal compound is selected from at least one of the chloride, nitrate, and acetate of the primary active metal and the secondary active metal; and / or, The solvent in the metal compound solution is water; and / or, The drying conditions are: drying temperature of 50~100℃ and drying time of 5~24h.
9. The preparation method according to claim 6, characterized in that, In method two: The pH value of the composite carrier dispersion is greater than 9; and / or, The heating and stirring conditions are: stirring at 60~120℃ for 0.5~10h.
10. The preparation method according to claim 6, characterized in that, The composite carrier is prepared by the following method: a component including at least one of inorganic oxides, diatomaceous earth, molecular sieves and graphene-coated nanodiamonds is added to a binder and mixed to form a composite.
11. The preparation method according to claim 10, characterized in that, The graphene-coated nanodiamond is obtained by calcining nanodiamond.
12. The preparation method according to claim 11, characterized in that, The calcination conditions are as follows: in a protective atmosphere, the calcination temperature is 900~1200℃, and the calcination time is 3~6h.
13. The C3 fraction selective hydrogenation catalyst according to any one of claims 1 to 4, or the C3 fraction selective hydrogenation catalyst obtained by the preparation method according to any one of claims 5 to 12, for the selective hydrogenation of propyne and propadiene in C3 fractions to produce propylene.
Citation Information
Patent Citations
Atomic-scale dispersed palladium-based nanometer diamond / graphene composite material catalyst, preparation method and applications thereof
CN109174085A
Catalyst for selective hydrogenation of acetylene hydrocarbon
CN1279126A
Selective hydrogenation catalyst of alkine and diolefin, preparation method and application
CN1958155A
Catalyst with composite carrier and preparation method thereof
CN118002108A
Catalyst for selective hydrogenation and preparation method and application thereof
CN118002114A