Pine tree-shaped bimetallic sulfide electrocatalytic material and preparation method and application thereof
By loading rose-shaped iron-cobalt bimetallic hydroxide onto nickel foam and confining the growth of nanospheres, followed by hydrothermal sulfidation to prepare pine-shaped FeCoS/NF materials, the problems of poor conductivity and few catalytic active sites in existing electrocatalytic materials in OER were solved, achieving highly efficient performance in the water electrolysis oxygen evolution reaction.
Patent Information
- Application Number
- CN202410415376.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-08
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-04-08
AI Technical Summary
Existing electrocatalytic materials suffer from poor conductivity, few catalytic active sites, cumbersome preparation steps, and scarce raw materials in the oxygen evolution reaction (OER) of water electrolysis. In particular, single metal sulfides such as cobalt-based and iron-based sulfides are difficult to meet the requirements of high-performance electrodes.
Using nickel foam as a substrate, rose-shaped iron-cobalt bimetallic hydroxide was loaded via hydrothermal reaction, followed by the confinement growth of nanospheres with organic ligands. Finally, pine-shaped bimetallic sulfide FeCoS/NF materials were prepared by hydrothermal sulfidation to form a three-dimensional porous structure to improve electrocatalytic performance.
The prepared FeCoS/NF material has small charge transfer resistance, large electrochemical surface area and good electrochemical stability, which significantly improves the catalytic activity and stability of OER and is suitable for industrial application in water electrolysis for hydrogen evolution.
Smart Images

Figure CN118477696B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of electrocatalytic material preparation technology, specifically to a pine-shaped bimetallic sulfide electrocatalytic material, its preparation method, and its application. Background Technology
[0002] Urbanization and industrialization are exacerbating the global energy crisis. To meet the world's growing energy demands, people are accelerating the use of non-renewable resources, but this also poses a significant obstacle to the development of the natural environment. Therefore, the development of clean and renewable energy sources is urgent. Electrochemical water splitting to produce efficient and pollution-free hydrogen and oxygen has been considered a promising method for generating green hydrogen sources as clean fuel alternatives. Electrocatalytic water splitting typically consists of two parts: the hydrogen evolution reaction (HER) at the cathode to produce hydrogen and the oxygen evolution reaction (OER) at the anode to produce oxygen. However, OER involves a four-electron transfer reaction and requires overcoming a high activation energy barrier, which has become one of the bottlenecks restricting hydrogen production from water electrolysis. Currently, the most ideal HER and OER catalysts are Pt-based and Ir / Ru-based noble metal catalysts, which can effectively improve OER efficiency, but their expensive and scarce nature prevents their large-scale commercial application. Transition metal sulfides are efficient and economical electrocatalytic materials, but they still have drawbacks such as poor conductivity and a small number of catalytic active sites. In particular, the electrochemical performance of single metal sulfides, such as cobalt-based and iron-based sulfides, is usually difficult to meet the requirements of high-performance electrodes.
[0003] Therefore, it is crucial to explore electrocatalytic materials that are high-performance, inexpensive, and stable. Summary of the Invention
[0004] To address the aforementioned technical problems, the present invention aims to provide a pine-like bimetallic sulfide electrocatalytic material, its preparation method, and its application. The electrocatalytic composite material of the present invention has low charge transfer resistance, large electrochemical surface area, and good electrochemical stability. Furthermore, the preparation method involved is simple and easy to operate, making it suitable for widespread application. This effectively solves the problems of cumbersome preparation steps, scarce raw materials, and poor electrocatalytic performance of existing OER electrocatalytic materials in electrocatalytic OER.
[0005] The technical solution of the present invention to solve the above-mentioned technical problems is as follows:
[0006] The first objective of this invention is to provide a pine-like bimetallic sulfide electrocatalytic material, wherein the pine-like bimetallic sulfide electrocatalytic material is FeCoS / NF and has a three-dimensional pine-like structure.
[0007] The beneficial effects of this invention are as follows: The FeCoS / NF electrocatalytic material prepared by this invention has a pine-tree-like nanoparticle structure. The pine-tree-like structure assembled from nanoparticles greatly increases the specific surface area of the material, exposing more electrochemical active sites, which facilitates the formation and diffusion of oxygen. Furthermore, it provides channels for electron movement on the phase surface through electron exchange between different valence bands, thereby generating higher catalytic activity. It also forms more electron transport pathways, and the three-dimensional porous structure provided by the nickel foam substrate facilitates electron conduction, further improving its electrocatalytic oxygen evolution performance.
[0008] A second objective of this invention is to provide a method for preparing a pine-shaped bimetallic sulfide electrocatalytic material, comprising the following steps:
[0009] S1. Using nickel foam as a base, cobalt salt, iron salt and surfactant are added and subjected to hydrothermal reaction to obtain rose-shaped iron-cobalt bimetallic hydroxide, namely FeCoOOH / NF;
[0010] S2. The FeCoOOH / NF and organic ligands were prepared by a room temperature static method to obtain an organometallic framework confined in the gap of iron-cobalt bimetallic hydroxide nanospheres, namely Fe-MOF-encapsulated FeCoOOH / NF, denoted as MIL / FeCoOOH / NF.
[0011] S3. Add the MIL / FeCoOOH / NF to the sulfide solution and obtain the pine-like bimetallic sulfide electrocatalytic material, namely FeCoS / NF, by hydrothermal sulfidation.
[0012] The beneficial effects of the above-mentioned scheme in this invention are as follows: First, using a hydrothermal reaction method, with nickel foam as a template and cobalt and iron salts as raw materials, and then adding a surfactant, a rose-shaped iron-nickel bimetallic oxide (FeCoOOH) is loaded onto nickel foam (NF); then, using it as a template and metal source, organic ligands are reacted with Fe... 3+ Ion bonding was used to confine the growth of Prussian blue analogue (MIL) nanospheres between FeCoOOH nanosheets to obtain MIL / FeCoOOH / NF; finally, a configurational transformation was achieved through hydrothermal sulfidation to obtain FeCoS / NF electrode material with a three-dimensional pine-tree-like hyperbranched structure.
[0013] Furthermore, step S1 includes the following specific steps:
[0014] Cobalt salt, iron salt, surfactant, and nickel foam were sequentially added to an aqueous solution and ultrasonically mixed. The mixture was then transferred to an autoclave and reacted at 120℃-130℃ for 6-8 hours. After the reaction was cooled to room temperature, the mixture was washed and freeze-dried to obtain FeCoOOH / NF.
[0015] The further beneficial effects of the present invention are as follows: using nickel foam as a template and cobalt salt and iron salt as raw materials, a hydrothermal reaction is carried out to grow cobalt ions and iron ions on the nickel foam, and then a surfactant is added to regulate the structure.
[0016] Furthermore, the molar mass ratio of the foamed nickel, the iron salt, and the cobalt salt is 1.7 mmol-1.8 mmol: 0.2-0.4 mmol: 0.4-0.5 mmol; the cobalt salt is at least one of cobalt nitrate hexahydrate, cobalt sulfate, and cobalt chloride; the iron salt is at least one of ferric nitrate nonahydrate, ferrous sulfate, and ferric chloride; and the surfactant is at least one of PVP, cetyltrimethylammonium bromide, and F127.
[0017] The further beneficial effect of the present invention is that it uses nickel foam, cobalt salt, and iron salt within the above-mentioned range per unit area mass to achieve the growth of rose-shaped iron-cobalt bimetallic hydroxide on nickel foam.
[0018] Furthermore, step S2 includes the following specific steps:
[0019] FeCoOOH / NF was soaked in a ferricyanide solution and an organic ligand was added. After being placed on a shaker at room temperature, it was washed with water and freeze-dried for 8-10 hours to obtain MIL / FeCoOOH / NF.
[0020] Further, in step S2, the ferricyanide in the ferricyanide solution is at least one of potassium ferricyanide, sodium ferricyanide, and cobalt ferricyanide; the organic ligand is at least one of mercaptoacetic acid, triethylamine, and ethylenediaminetetraacetic acid (EDTA); the mass ratio of the organic ligand, the ferricyanide solution, and the iron-cobalt bimetallic hydroxide is (33-34) g: (1-2) g: (0.01-0.5) g.
[0021] The further beneficial effect of the present invention is that the electrocatalytic activity of the material is improved by regulating the quality of the organic ligand, ferricyanide solution, and iron-cobalt bimetallic hydroxide.
[0022] Furthermore, the room temperature standing method in step S2 specifically involves soaking at room temperature for 24-28 hours.
[0023] The further beneficial effects of the present invention are as follows: the present invention combines organic ligands with Fe... 3+ Ion bonding was used to confine the growth of Prussian blue analogue (MIL) nanospheres between FeCoOOH nanosheets, resulting in MIL / FeCoOOH / NF.
[0024] Furthermore, the hydrothermal sulfidation method described in step S3 specifically involves placing the prepared MIL / FeCoOO H / NF into a sulfide solution and hydrothermally reacting it at 180℃-200℃ for 6-8 hours.
[0025] The further beneficial effect of the present invention is that, through hydrothermal sulfidation, the material undergoes a configurational transformation to obtain a pine-shaped FeCoS / NF electrode material with electrocatalytic properties.
[0026] Furthermore, the sulfide in the sulfide solution is at least one of thioacetamide, sulfur, and thiourea; the ratio of MIL / FeCoOOH / NF to the sulfide solution is 2-3g:1-2g.
[0027] The third objective of this invention is to provide an application of a pine-shaped bimetallic sulfide electrocatalytic material, which is used in the electrolysis of water to produce hydrogen.
[0028] The beneficial effects of the above-mentioned scheme in this invention are: the electrocatalytic material prepared by this invention has a small charge transfer resistance, a large electrochemical surface area and good electrochemical stability, and the preparation method is simple and easy to operate, suitable for promotion and application, and has strong application potential in industry. When applied to the electrolysis of water to generate hydrogen, it can be stably used for OER in a strongly alkaline medium for a long time. Attached Figure Description
[0029] Figure 1 The diagram shows the working principle of the FeCoS / NF material of the present invention; (a) is the working principle diagram of the FeCoS / NF material in water electrolysis; and (b) is the working principle diagram of the FeCoS / NF material in a zinc-air battery.
[0030] Figure 2 This is an open-circuit voltage diagram of the FeCoS / NF material in a zinc-air battery according to Example 1 of the present invention.
[0031] Figure 3 The following are SEM images of Example 1 of the present invention: (a) SEM image of FeCoOOH / NF material prepared in step (1) of Example 1 at 5 μm; (b) SEM image of MIL / FeCoOOH / NF material prepared in step (2) of Example 1 at 5 μm; (c) SEM image of FeCoS / NF material prepared in step (3) of Example 1 at 5 μm; (d) SEM image of FeCoOOH / NF material prepared in step (1) of Example 1 at 2 μm; (e) SEM image of MIL / FeCoOOH / NF material prepared in step (2) of Example 1 at 2 μm; (f) SEM image of FeCoS / NF material prepared in step (3) of Example 1 at 2 μm.
[0032] Figure 4 This is the XRD pattern of Embodiment 1 of the present invention.
[0033] Figure 5 The images show the Tafel slopes of the FeCoS / NF material of Example 2, the FeCoOOH-S / NF material of Comparative Example 1, the NF-S material of Comparative Example 2, the MIL / FeCoOOH / NF material of Comparative Example 3, and the FeCoOOH / NF material of Comparative Example 4.
[0034] Figure 6 The Nyquist curves of the FeCoS / NF material of Example 2, the FeCoOOH-S / NF material of Comparative Example 1, the NF-S material of Comparative Example 2, the MIL / FeCoOOH / NF material of Comparative Example 3, and the FeCoOOH / NF material of Comparative Example 4 are obtained after fitting.
[0035] Figure 7 The bilayer capacitance (C) of the FeCoS / NF material of Example 3, the FeCoOOH-S / NF material of Comparative Example 5, the NF-S material of Comparative Example 6, the MIL / FeCoOOH / NF material of Comparative Example 7, and the FeCoOOH / NF material of Comparative Example 8 are shown. dl )picture.
[0036] Figure 8 This is a static stability test curve of the FeCoS / NF material in Example 3 of the present invention. Detailed Implementation
[0037] The principles and features of this invention are described below. The examples given are for illustrative purposes only and are not intended to limit the scope of the invention. Where specific techniques or conditions are not specified in the embodiments, they should be performed according to the techniques or conditions described in the literature in this field, or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased through legitimate channels.
[0038] Example 1: Preparation of FeCoS / NF
[0039] (1) A piece of 30mm×10mm, 0.1051g of nickel foam was ultrasonically treated in 3M HCl solution for 10min to remove possible oxides on the surface. Then it was rinsed with ethanol and ultrasonically treated for 10min. Then it was ultrasonically treated with pure water for 5min. The ultrasonic treatment in pure water was repeated twice. After drying, pretreated nickel foam was obtained. 0.2mmol Fe(NO3)3·9H2O, 0.4mmol Co(NO3)2·6H2O, 0.22g NH4F, 0.24g NH4Ac, 0.2g PVP and pretreated nickel foam were placed in 30mL of pure water and ultrasonically dispersed evenly. Then it was transferred to a 50mL autoclave and reacted in a muffle furnace at 120℃ for 6h. After the reaction was completed, it was cooled to room temperature, washed with deionized water, and then freeze-dried at -80℃--100℃ for 8h to obtain FeCoOOH / NF.
[0040] (2) A 30mm×10mm, 0.1065g piece of FeCoOOH / NF was soaked in 50mL of 0.05M potassium ferricyanide solution and 10μL of 82.908g / L mercaptoacetic acid solution was added. Then, it was placed on a shaker at room temperature for 24h. The nickel foam was removed, washed with water, and freeze-dried at -80℃ for 8h to obtain MIL / FeCoOOH / NF.
[0041] (3) Add a 30mm×10mm, 0.1079g piece of MIL / FeCoOOH / NF to 30mL of 0.05M thioacetamide solution, then put it into a 50mL reaction vessel and react at 180℃ for 8h. After the reaction is cooled to room temperature, take it out, wash and dry it at room temperature to obtain FeCoS / NF.
[0042] Example 2: Preparation of FeCoS / NF
[0043] (1) A 30mm×10mm, 0.1011g piece of nickel foam was ultrasonically treated in 3M HCl solution for 10min to remove any possible oxides on the surface. Then it was rinsed with ethanol and ultrasonically treated for 10min, followed by ultrasonic treatment with pure water for 5min. This ultrasonic treatment in pure water was repeated twice. After drying, pretreated nickel foam was obtained. 0.2mmol Fe(NO3)3·9H2O, 0.4mmol Co(NO3)2·6H2O, 0.22g NH4F, 0.24g NH4Ac, 0.2g hexadecyltrimethylammonium bromide and the pretreated nickel foam were sequentially placed in 30mL of aqueous solution and ultrasonically dispersed evenly. The mixture was then transferred to a 50mL autoclave and reacted in a muffle furnace at 120℃ for 6h. After the reaction was cooled to room temperature, the mixture was removed, washed with deionized water, and then freeze-dried for 8h to obtain FeCoOOH / NF.
[0044] (2) A 30mm×10mm, 0.1023g piece of FeCoOOH / NF was soaked in 50mL of 0.05M sodium ferricyanide solution and 10μL of 91.017g / L triethylamine solution was added. The mixture was then placed on a shaker at room temperature for 24h. The nickel foam was removed, washed with water, and freeze-dried at -80℃ for 8h to obtain MIL / FeCoOOH / NF.
[0045] (3) Place a 30mm×10mm, 0.1031g MIL / FeCoOOH / NF into 30mL of 0.05M sulfur solution, then place it into a 50mL reaction vessel and react at 180℃ for 8h. After the reaction is cooled to room temperature, take it out, wash and dry it at room temperature to obtain FeCoS / NF.
[0046] Example 3: Preparation of FeCoS / NF
[0047] (1) A piece of 30mm×10mm, 0.1075g of nickel foam was ultrasonically treated in 3M HCl solution for 10min to remove possible oxides on the surface. Then it was rinsed with ethanol and ultrasonically treated for 10min. Then it was ultrasonically treated with pure water for 5min. The ultrasonic treatment in pure water was repeated twice. After drying, pretreated nickel foam was obtained. 0.2mmol Fe(NO3)3·9H2O, 0.4mmol Co(NO3)2·6H2O, 0.22g NH4F, 0.24g NH4Ac, 0.2g F127 and pretreated nickel foam were placed in 30mL of pure water and ultrasonically dispersed evenly. Then it was transferred to a 50mL autoclave and reacted in a muffle furnace at 120℃ for 6h. After the reaction was completed, it was cooled to room temperature, washed with deionized water, and then freeze-dried at -80--100℃ for 8h to obtain FeCoOOH / NF.
[0048] (2) A 30mm×10mm, 0.1085g FeCoOOH / NF was soaked in 50mL of 0.05M cobalt ferricyanide solution and 10μL of 263.025g / L ethylenediaminetetraacetic acid solution was added. The mixture was then placed on a shaker at room temperature for 24h. The nickel foam was removed, washed with water, and freeze-dried at -80℃ for 8h to obtain MIL / FeCoOOH / NF.
[0049] (3) Add a 30mm×10mm, 0.1099g piece of MIL / FeCoOOH / NF to 30mL of 0.05M thiourea solution, then put it into a 50mL reaction vessel and react at 180℃ for 8h. After the reaction is cooled to room temperature, take it out, wash and dry it at room temperature to obtain FeCoS / NF.
[0050] Comparative Example 1: Preparation of FeCoOOH-S / NF composite material
[0051] The only difference between this comparative example and Example 2 is the absence of step (2) in the preparation process; all other steps and materials used are the same. The specific steps are as follows:
[0052] (1) A 30mm×10mm, 0.1033g piece of nickel foam was ultrasonically treated in 3M HCl solution for 10min to remove any possible oxides on the surface. Then it was rinsed with ethanol and ultrasonically treated for 10min, followed by ultrasonic treatment with pure water for 5min. This ultrasonic treatment in pure water was repeated twice. After drying, pretreated nickel foam was obtained. 0.2mmol Fe(NO3)3·9H2O, 0.4mmol Co(NO3)2·6H2O, 0.22g NH4F, 0.24g NH4Ac, 0.2g hexadecyltrimethylammonium bromide and pretreated nickel foam were sequentially placed in 30mL of pure water and ultrasonically dispersed evenly. The mixture was then transferred to a 50mL autoclave and reacted in a muffle furnace at 120℃ for 6h. After the reaction was cooled to room temperature, the mixture was washed with deionized water and then freeze-dried for 8h to obtain FeCoOOH / NF.
[0053] (2) Place a 30mm×10mm, 0.1041g FeCoOOH / NF into 30mL of 0.05M sulfur solution, then place it into a 50mL reaction vessel and react at 180℃ for 8h. After the reaction is cooled to room temperature, take it out, wash and dry it at room temperature to obtain FeCoOOH-S / NF.
[0054] Comparative Example 2: Preparation of NF-S composite materials
[0055] A 30mm × 10mm, 0.1051g piece of nickel foam was ultrasonically treated in 3M HCl solution for 10 minutes to remove any possible oxides on the surface. Then, it was rinsed with ethanol and ultrasonically treated for 10 minutes, followed by ultrasonic treatment with pure water for 5 minutes. This ultrasonic treatment in pure water was repeated twice. After drying, pretreated nickel foam was obtained. The pretreated NF was placed in 30mL of 0.05M sulfur solution and then placed in a 50mL reactor. The reactor was reacted at 180℃ for 8 hours. After cooling to room temperature, the NF-S was obtained by cold washing and drying at room temperature.
[0056] Comparative Example 3: Preparation of MIL / FeCoOOH / NF composite material
[0057] The only difference between this comparative example and Example 2 is the absence of step (3) in the preparation process. The remaining steps and materials used are the same, as follows:
[0058] (1) A piece of nickel foam with a diameter of 30 mm × 10 mm and a mass of 0.1022 g was ultrasonically treated in 3M HCl solution for 10 min to remove any possible oxides on the surface. Then, it was rinsed with ethanol and ultrasonically treated for 10 min, followed by ultrasonic treatment with pure water for 5 min. This ultrasonic treatment in pure water was repeated twice. After drying, pretreated nickel foam was obtained. 0.2 mmol Fe(NO3)3·9H2O, 0.4 mmol Co(NO3)2·6H2O, 0.22 g NH4F, 0.24 g NH4Ac, 0.2 g hexadecyltrimethylammonium bromide and pretreated nickel foam were sequentially placed in 30 mL of aqueous solution and ultrasonically dispersed evenly. The mixture was then transferred to a 50 mL autoclave and reacted in a muffle furnace at 120 °C for 6 h. After the reaction was cooled to room temperature, the mixture was removed, washed with deionized water, and then freeze-dried for 8 h to obtain FeCoOOH / NF.
[0059] (2) A 30mm×10mm, 0.1031g FeCoOOH / NF was soaked in 50mL of 0.05M sodium ferricyanide solution and 10μL of 91.017g / L triethylamine solution was added. The mixture was then placed on a shaker at room temperature for 24h. The nickel foam was removed, washed with water, and freeze-dried at -80℃ for 8h to obtain MIL / FeCoOOH / NF.
[0060] Comparative Example 4: Preparation of FeCoOOH / NF Composite Material
[0061] The only difference between this comparative example and Example 2 is the absence of steps (2) and (3) in the preparation process. The remaining steps and materials used are the same. The specific steps are as follows:
[0062] (1) A 30mm × 10mm piece of nickel foam with a mass of 0.1051g was ultrasonically treated in 3M HCl solution for 10min to remove any possible oxides on the surface. Then, it was rinsed with ethanol and ultrasonically treated for 10min, followed by ultrasonic treatment with pure water for 5min. This ultrasonic treatment in pure water was repeated twice. After drying, pretreated nickel foam was obtained. 0.2mmol Fe(NO3)3·9H2O, 0.4mmol Co(NO3)2·6H2O, 0.22g NH4F, 0.24g NH4Ac, 0.2g hexadecyltrimethylammonium bromide and the pretreated nickel foam were sequentially placed in 30mL of aqueous solution and ultrasonically dispersed evenly. The mixture was then transferred to a 50mL autoclave and reacted in a muffle furnace at 120℃ for 6h. After cooling to room temperature, the mixture was washed with deionized water and then freeze-dried for 8h to obtain FeCoOOH / NF.
[0063] Comparative Example 5: Preparation of FeCoOOH-S / NF Composite Material
[0064] The only difference between this comparative example and Example 3 is the absence of step (2) in the preparation process. The remaining steps and materials used are the same. The specific steps are as follows:
[0065] (1) A piece of 30mm×10mm nickel foam with a mass of 0.1045g was ultrasonically treated in 3M HCl solution for 10min to remove possible oxides on the surface. Then it was rinsed with ethanol and ultrasonically treated for 10min, and then ultrasonically treated with pure water for 5min. The ultrasonic treatment in pure water was repeated twice. After drying, pretreated nickel foam was obtained. 0.2mmol Fe(NO3)3·9H2O, 0.4mmol Co(NO3)2·6H2O, 0.22g NH4F, 0.24g NH4Ac, 0.2g F127 and pretreated nickel foam were placed in 30mL of ion-soluble aqueous solution and ultrasonically dispersed evenly. The solution was then transferred to a 50mL autoclave and reacted in a muffle furnace at 120℃ for 6h. After the reaction was completed, the solution was cooled to room temperature, washed with deionized water, and then freeze-dried at -80 to -100℃ for 8h to obtain FeCoOOH / NF.
[0066] (2) Add a 30mm×10mm, 0.1055g piece of FeCoOOH / NF to 30mL of 0.05M thiourea solution, then put it into a 50mL reaction vessel and react at 180℃ for 8h. After the reaction is cooled to room temperature, take it out, wash and dry it at room temperature to obtain FeCoOOH-S / NF.
[0067] Comparative Example 6: Preparation of NF-S composite materials
[0068] A 30mm × 10mm piece of nickel foam with a mass of 0.1051g was ultrasonically treated in 3M HCl solution for 10min to remove any possible oxides on the surface. Then, it was rinsed with ethanol and ultrasonically treated for 10min, followed by ultrasonic treatment with pure water for 5min. This ultrasonic treatment in pure water was repeated twice. After drying, pretreated nickel foam was obtained. The pretreated NF was added to 30mL of 0.05M thiourea solution and then placed in a 50mL reactor. The reactor was reacted at 180℃ for 8h. After cooling to room temperature, the reactor was removed, cold washed and dried at room temperature to obtain NF-S.
[0069] Comparative Example 7: Preparation of MIL / FeCoOOH / NF composite material
[0070] The only difference between this comparative example and Example 3 is the absence of step (3) in the preparation process; the remaining steps and materials used are the same. The specific steps are as follows:
[0071] (1) A piece of 30mm×10mm, 0.1067g of nickel foam was ultrasonically treated in 3M HCl solution for 10min to remove possible oxides on the surface. Then it was rinsed with ethanol and ultrasonically treated for 10min, and then ultrasonically treated with pure water for 5min. The ultrasonic treatment in pure water was repeated twice. After drying, pretreated nickel foam was obtained. 0.2mmol Fe(NO3)3·9H2O, 0.4mmol Co(NO3)2·6H2O, 0.22g NH4F, 0.24g NH4Ac, 0.2g F127 and pretreated nickel foam were placed in 30mL of pure water and ultrasonically dispersed evenly. The mixture was then transferred to a 50mL autoclave and reacted in a muffle furnace at 120℃ for 6h. After the reaction was completed, the mixture was cooled to room temperature, washed with deionized water, and then freeze-dried at -80℃ to -100℃ for 8h to obtain FeCoOOH / NF.
[0072] (2) A 30mm×10mm, 0.1075g FeCoOOH / NF was soaked in 50mL of 0.05M cobalt ferricyanide solution and 10μL of 263.025g / L ethylenediaminetetraacetic acid solution was added. The mixture was then placed on a shaker at room temperature for 24h. The nickel foam was removed, washed with water, and freeze-dried at -80℃ for 8h to obtain MIL / FeCoOOH / NF.
[0073] Comparative Example 8: Preparation of FeCoOOH / NF Composite Material
[0074] The only difference between this comparative example and Example 3 is the absence of steps (2) and (3) in the preparation process. The remaining steps and materials used are the same. The specific steps are as follows:
[0075] (1) A piece of 30mm×10mm, 0.1051g of nickel foam was ultrasonically treated in 3M HCl solution for 10min to remove any possible oxides on the surface. Then it was rinsed with ethanol and ultrasonically treated for 10min, and then ultrasonically treated with pure water for 5min. The ultrasonic treatment in pure water was repeated twice. After drying, pretreated nickel foam was obtained. 0.2mmol Fe(NO3)3·9H2O, 0.4mmol Co(NO3)2·6H2O, 0.22g NH4F, 0.24g NH4Ac, 0.2g F127 and pretreated nickel foam were placed in 30mL of pure water and ultrasonically dispersed evenly. The mixture was then transferred to a 50mL autoclave and reacted in a muffle furnace at 120℃ for 6h. After the reaction was completed, the mixture was cooled to room temperature, washed with deionized water, and then freeze-dried at -80℃ to -100℃ for 8h to obtain FeCoOOH / NF.
[0076] Performance characterization test:
[0077] 1. Open circuit voltage test
[0078] Using the FeCoS / NF prepared in Example 1 as the cathode, a zinc sheet as the anode, and 6M KOH solution, 0.3M ZnCl2 solution, and 0.05M citric acid solution as electrolytes, a liquid zinc-air battery was assembled in a mold and tested at a scan rate of 0.005 mV·s. -1 The open-circuit voltage was tested under a test time of 10000s, and the test results are as follows. Figure 2 As shown:
[0079] Depend on Figure 2 Therefore, the open-circuit voltage of the zinc-air battery is 1.2V.
[0080] 2. SEM, TEM, and XRD tests
[0081] The FeCoS / NF prepared in Example 1 was analyzed and tested using scanning electron microscopy (Sigma-HD) and transmission electron microscopy (JEM-ARF200F) via SEM, TEM, and XRD. The results of SEM and TEM analysis are as follows: Figure 3 , Figure 4 As shown.
[0082] Depend on Figure 3 , Figure 4 We can obtain:
[0083] Figure 3 (a) is a SEM image of the FeCoOOH / NF material prepared in step (1) of Example 1 at 5 μm; Figure 3 (b) is a SEM image of the MIL / FeCoOOH / NF material prepared in step (2) of Example 1 at 5 μm; Figure 3 (c) is a SEM image of the FeCoS / NF material prepared in step (3) of Example 1 at 5 μm; Figure 3 (d) is a SEM image of the FeCoOOH / NF material prepared in step (1) of Example 1 at 2 μm; Figure 3 (e) is a SEM image of the MIL / FeCoOOH / NF material prepared in step (2) of Example 1 at 2 μm; Figure 3 (f) is a SEM image of the FeCoS / NF material prepared in step (3) of Example 1 at 2 μm.
[0084] from Figure 3 As can be seen, FeCoS / NF has a pine-like nanoparticle structure. This pine-like structure assembled from nanoparticles greatly increases the specific surface area of the material, accelerates electrolyte permeation and gas desorption, thereby improving its OER activity.
[0085] Figure 4The XRD pattern of FeCoS / NF in Example 1 is shown below. Figure 4 The successful synthesis of FeCoS / NF can be seen.
[0086] 3. Tafel slope and Nyquist curve
[0087] A series of electrochemical performance tests were conducted on the FeCoS / NF material of Example 2, the FeCoOOH-S / NF material of Comparative Example 1, the NF-S material of Comparative Example 2, the MIL / FeCoOOH / NF material of Comparative Example 3, and the FeCoOOH / NF material of Comparative Example 4 using a three-electrode system via an electrochemical workstation (CHI760E).
[0088] Test method:
[0089] (1) Cut the FeCoS / NF material of Example 2, the FeCoOOH-S / NF material of Comparative Example 1, the NF-S material of Comparative Example 2, the MIL / FeCoOOH / NF material of Comparative Example 3, and the FeCoOOH / NF material of Comparative Example 4 into 0.5cm×0.5cm sizes for later use.
[0090] (2) Under conditions of 25±0.3℃, NF was used as the substrate, 1M KOH solution with pH=14 was used as the electrolyte, a saturated calomel electrode was used as the reference electrode, and a graphite rod was used as the counter electrode. The KOH solution was purged with nitrogen for 30 min before each electrochemical experiment. All electrode materials were activated by cyclic activation with an activation voltage window of -1.5 to 0.6 V versus RHE before each test, and then the scan rate was 2 mV·s. -1 The Tafel slope was obtained by fitting the polarization curve using the linear sweep voltammetry method under the condition that the OER test range is 0-0.6V.
[0091] (3) Subsequently, under the conditions of a frequency range of 100KHz-0.01Hz and a step voltage of 5mV, the impedance data was fitted using ZSimpWin software.
[0092] Test results are as follows Figure 5 , Figure 6 As shown:
[0093] Figure 5 Tafel slope plots for the FeCoS / NF material of Example 2, the FeCoOOH-S / NF material of Comparative Example 1, the NF-S material of Comparative Example 2, the MIL / FeCoOOH / NF material of Comparative Example 3, and the FeCoOOH / NF material of Comparative Example 4; from Figure 5 It can be seen that FeCoS / NF has the lowest Tafel slope, at only 37 mV·dec.-1 It is evident that FeCoS / NF exhibits the least electron transfer barrier and thus the best catalytic performance.
[0094] Figure 6 The Nyquist plots are for the FeCoS / NF material of Example 2, the FeCoOOH-S / NF material of Comparative Example 1, the NF-S material of Comparative Example 2, the MIL / FeCoOOH / NF material of Comparative Example 3, and the FeCoOOH / NF material of Comparative Example 4, after fitting. Figure 6 This indicates that FeCoS / NF has the lowest impedance, only 1.97Ω, and possesses excellent electron transfer capability, providing rapid charge transfer motive force for the OER reaction. The interfacial interactions generated during its formation process also give it excellent electrical conductivity.
[0095] 4. Double-layer capacitance value (C) dl Static stability test
[0096] The bilayer capacitance (C0) of the FeCoS / NF material in Example 3, the FeCoOOH-S / NF material in Comparative Example 5, the NF-S material in Comparative Example 6, the MIL / FeCoOOH / NF material in Comparative Example 7, and the FeCoOOH / NF material in Comparative Example 8 was measured using an electrochemical workstation (CHI760E) with a three-electrode system. dl Electrochemical performance testing for static stability.
[0097] Test method:
[0098] (1) Cut the FeCoS / NF material of Example 3, the FeCoOOH-S / NF material of Comparative Example 5, the NF-S material of Comparative Example 6, the MIL / FeCoOOH / NF material of Comparative Example 7, and the FeCoOOH / NF material of Comparative Example 8 into 0.5cm×0.5cm sizes for later use.
[0099] (2) At 25±0.3℃, NF was used as the substrate, 1M KOH aqueous solution with pH=14 was used as the electrolyte, a saturated calomel electrode was used as the reference electrode, and a graphite rod was used as the counter electrode. The KOH solution was purged with nitrogen for 30 min before each electrochemical experiment. All electrode materials were activated by cyclic activation with an activation voltage window of -1.5 to 0.6 V versus RHE before each test, and then subjected to CV at different scan rates (20 mV·s) in the non-Radida reaction range. -1 400mV·s -1 60mV·s -1 80mV·s -1 100mV·s -1The scan is performed below, and C is calculated. dl value;
[0100] (3) At 100mV·s -1 The scan rate and 10 mA cm -2 CP, current density is 10 mA cm -2 Under certain conditions, the static stability test curve was obtained by performing 2000 consecutive cyclic voltammetric scans on the FeC oS / NF material of Example 3 between -0.2V and 0.2V (relative to RHE).
[0101] Test results are as follows Figure 7 , Figure 8 As shown:
[0102] Figure 7 The bilayer capacitance (C) of the FeCoS / NF material in Example 3, the FeCoOOH-S / NF material in Comparative Example 5, the NF-S material in Comparative Example 6, the MIL / FeCoOOH / NF material in Comparative Example 7, and the FeCoOOH / NF material in Comparative Example 8 are shown. dl (Figure; from) Figure 7 It can be seen from this that the C of FeCoS / NF dl The value is the highest, reaching 3.4 mF·cm. -2 This indicates that FeCoS / NF has many electrochemical active sites and a large electrochemical surface area; Figure 8 The graph shows the static stability test results of the FeCoS / NF material in Example 3. Figure 8 As can be seen, after 24 hours of continuous testing, the potential of FeCoS / NF hardly changed, and it can be stably used in OER in a strongly alkaline medium for a long time.
[0103] In summary, the three-dimensional pine-structured FeCoS / NF nanomaterials prepared according to the method of this invention have good OER catalytic performance and good electrochemical stability in alkaline electrolytes, and have strong application potential in industry.
[0104] Although embodiments of the present invention have been shown and described above, it is understood that the above embodiments are exemplary and should not be construed as limiting the present invention. Those skilled in the art can make changes, modifications, substitutions and variations to the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a pine-shaped bimetallic sulfide electrocatalytic material, characterized in that, The preparation method includes the following steps: S1. Using nickel foam as a base, cobalt salt, iron salt and surfactant are added and subjected to hydrothermal reaction to obtain rose-shaped iron-cobalt bimetallic hydroxide. S2. The rose-shaped iron-cobalt bimetallic hydroxide and organic ligands were combined by a room temperature static method to prepare nanospheres with an organometallic framework confined within the gaps of the iron-cobalt bimetallic hydroxide. S3. The nanospheres confined within the gaps of the rose-shaped bimetallic hydroxide by the organometallic framework are added to a sulfide solution, and a pine-shaped bimetallic sulfide electrocatalytic material is obtained by hydrothermal sulfidation. Step S2 includes the following specific steps: Rose-shaped iron-cobalt bimetallic hydroxide was immersed in ferricyanide solution, and organic ligands were added. After being placed on a shaker at room temperature, it was taken out, washed with water, and freeze-dried for 8-10 hours to obtain nanospheres confined in the gaps of the rose-shaped bimetallic hydroxide by an organometallic framework. The pine-tree-like bimetallic sulfide electrocatalytic material is FeCoS / NF, which has a three-dimensional pine-tree-like structure. The molar ratio of the foamed nickel, the iron salt, and the cobalt salt is 1.7-1.8 mmol: 0.2-0.4 mmol: 0.4-0.5 mmol; the cobalt salt is at least one of cobalt nitrate hexahydrate, cobalt sulfate, and cobalt chloride; the iron salt is at least one of ferric nitrate nonahydrate, ferrous sulfate, and ferric chloride; and the surfactant is at least one of PVP, hexadecyltrimethylammonium bromide, and F127. The ferricyanide in the ferricyanide solution is at least one of potassium ferricyanide, sodium ferricyanide, and cobalt ferricyanide; the organic ligand is at least one of mercaptoacetic acid, triethylamine, and ethylenediaminetetraacetic acid; the mass ratio of the organic ligand, the ferricyanide solution, and the iron-cobalt bimetallic hydroxide is (33-34) g : (1-2) g : (0.01-0.5) g; The room temperature standing method in step S2 specifically involves soaking for 24-28 hours at room temperature; The hydrothermal sulfidation method described in step S3 specifically involves placing the nanospheres, which are confined within the gaps of an iron-cobalt bimetallic hydroxide and confined within the organometallic framework, into a sulfide solution and hydrothermally reacting them at 180℃-200℃ for 6-8 hours.
2. The method for preparing a pine-shaped bimetallic sulfide electrocatalytic material according to claim 1, characterized in that, Step S1 includes the following specific steps: Cobalt salt, iron salt, surfactant, and nickel foam were sequentially added to an aqueous solution and ultrasonically mixed. The mixture was then transferred to an autoclave and reacted at 120℃-130℃ for 6-8 hours. After the reaction was cooled to room temperature, the mixture was washed and freeze-dried to obtain a rose-shaped iron-cobalt bimetallic hydroxide.
3. The method for preparing a pine-shaped bimetallic sulfide electrocatalytic material according to claim 1, characterized in that, The sulfide in the sulfide solution is at least one of thioacetamide, sulfur, and thiourea; the ratio of the amount of nanospheres confined in the gaps of the iron-cobalt bimetallic hydroxide framework to the amount of sulfide solution is 2-3g:1-2g.
4. The application of a pine-shaped bimetallic sulfide electrocatalytic material, characterized in that, The pine-shaped bimetallic sulfide electrocatalytic material prepared by the preparation method according to any one of claims 1 to 3 is applied to hydrogen evolution in water electrolysis.
Citation Information
Patent Citations
Prussian blue derivative Fe-Co-Ni sulfide and preparation method and application thereof
CN108091875A
Foamed nickel loaded sulfide bifunctional electrocatalyst as well as preparation method and application thereof
CN115747868A