A method for producing silicon carbide

By layering silicon-rich and carbon-rich raw materials and controlling heating conditions, the problems of raw material waste and container damage caused by silicon vapor enrichment are solved, achieving efficient and low-cost silicon carbide production.

CN118479480BActive Publication Date: 2026-11-20BYD CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310131252.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-10
Publication Date
2026-11-20
Estimated Expiration
2043-02-10

AI Technical Summary

Technical Problem

In current silicon carbide production, the silicon powder particles are relatively large, causing silicon vapor to accumulate at the top of the crucible and react with carbon, resulting in raw material waste and damage to the reaction vessel, thus increasing production costs.

Method used

Silicon-rich raw materials are laid at the bottom of the reaction vessel, and carbon-rich raw materials are laid on top. Layered heating allows silicon and carbon to react fully, reducing silicon vapor escape, material waste, and vessel wear.

Benefits of technology

It effectively reduces the accumulation and leakage of silicon vapor at the top of the reaction vessel, reduces raw material loss and vessel corrosion, lowers production costs, and improves the quality and production efficiency of silicon carbide.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004086864800000071
    Figure BDA0004086864800000071
Patent Text Reader

Abstract

The application provides a preparation method of silicon carbide, which can greatly reduce the loss of reaction containers and other materials and the waste of raw materials caused by silicon sublimation in the production process of silicon carbide, thereby greatly reducing the production cost of silicon carbide while ensuring the quality of silicon carbide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of silicon carbide preparation technology, specifically to a method for preparing silicon carbide. Background Technology

[0002] Silicon carbide is one of the most promising semiconductor materials. The production of silicon carbide mainly relies on solid-state synthesis. In general, silicon powder and carbon powder are mixed evenly and then placed in a crucible for firing to prepare silicon carbide. However, the particle size of silicon powder is relatively large. After the surface of silicon powder particles reacts with carbon powder, the unreacted silicon inside the particles will sublimate at high temperature. Silicon vapor will accumulate at the top of the crucible and react with carbon elements in the crucible lid, resulting in waste of raw materials and loss of reaction vessels and other materials (e.g., crucible, insulation materials). Summary of the Invention

[0003] In view of this, this application provides a method for preparing silicon carbide, which can greatly reduce the loss of reaction vessels and other materials and the waste of raw materials caused by silicon sublimation during the silicon carbide production process, thereby greatly reducing the production cost of silicon carbide while ensuring its quality.

[0004] The first aspect of this application provides a method for preparing silicon carbide, comprising:

[0005] (1) Loading raw materials into a reaction vessel, the raw materials including silicon-rich raw materials and carbon-rich raw materials; wherein, the silicon-rich raw materials are laid at the bottom of the reaction vessel and the carbon-rich raw materials are filled on the surface of the silicon-rich raw materials.

[0006] The silicon-rich raw material includes silicon powder and carbon powder, and the molar amount of silicon in the silicon-rich raw material is greater than the molar amount of carbon; the carbon-rich raw material includes silicon powder and carbon powder, and the molar amount of carbon in the carbon-rich raw material is greater than the molar amount of silicon.

[0007] (2) Place the reaction vessel containing the raw material in a heating device, evacuate the heating device, and then heat it to obtain silicon carbide.

[0008] The above preparation method is simple, highly controllable, and has high production efficiency, enabling large-scale industrial production.

[0009] Optionally, in the silicon-rich raw material, the molar ratio of carbon to silicon is 1:(1.1-1.3).

[0010] Optionally, in the carbon-rich raw material, the molar ratio of silicon to carbon is 1:(1.04-1.27).

[0011] Optionally, in the carbon-rich raw material, the molar ratio of silicon to carbon is 1:(1.10-1.27).

[0012] Optionally, the silicon-rich raw material comprises 30%-50% by mass, based on the total mass of the raw material.

[0013] Optionally, in the raw material, the molar ratio of carbon to silicon is 1:1.

[0014] Optionally, the reaction vessel is a graphite crucible.

[0015] Optionally, the inner wall of the graphite crucible is further provided with graphite paper.

[0016] Optionally, during the heating process, the graphite crucible is wrapped with carbon fiber felt.

[0017] Optionally, the heating includes:

[0018] a) Evacuate the heating device until the relative pressure inside is less than or equal to 10. -5 After mbar, the temperature is increased to 500-800℃ at a heating rate of 15℃ / min-20℃ / min;

[0019] b) Under the condition that the relative pressure inside the heating device is less than or equal to 10 mbar, the temperature is further increased to 1300-1400℃ at a rate of 15℃ / min-20℃ / min. Inert gas is introduced into the heating device until the relative pressure inside the heating device is 800mbar-1000mbar. At the same time as the inert gas is introduced, the temperature is increased to 2100℃-2400℃ at a rate of 8-10℃ / min and held for 5h-10h to obtain silicon carbide.

[0020] Optionally, after step b), the heating further includes step c): evacuating the heating device to a relative pressure less than or equal to 30 mbar, then introducing inert gas again to a relative pressure of 500 mbar-800 mbar inside the heating device, and then cooling it down.

[0021] Optionally, in the heating step (1), at least one gas scrubbing process is performed simultaneously with the heating, the gas scrubbing process including:

[0022] Inert gas is introduced into the heating device until the relative pressure inside the heating device is 500mbar-800mbar, and the pressure is maintained for 10min-15min. Then, a vacuum is drawn until the relative pressure inside the heating device is less than or equal to 10mbar.

[0023] Optionally, the raw materials include high-purity carbon powder and high-purity silicon powder.

[0024] Optionally, the method further includes crushing and screening the silicon carbide to obtain silicon carbide powder. Detailed Implementation

[0025] In traditional methods, silicon carbide is typically prepared by directly heating a homogeneously mixed mixture of silicon powder and carbon powder. However, the silicon powder particles are relatively large, and the silicon on the surface of the particles, after reacting with carbon to form silicon carbide, hinders the reaction between silicon and carbon inside the silicon powder particles. Further heating can melt and release the silicon inside the particles, but it can also lead to sublimation, resulting in accumulation at the top of the reaction vessel (usually a graphite crucible). There, it reacts with the carbon inside the crucible, and the products deposit on the crucible lid. This can even cause silicon vapor leakage, leading to raw material loss and corrosion of the graphite crucible and other materials (e.g., the carbon fiber felt used for insulation around the crucible). This increases the production cost of silicon carbide. To address these problems, this application provides a method for preparing silicon carbide, including:

[0026] S01. Load raw materials into a reaction vessel, the raw materials including silicon-rich raw materials and carbon-rich raw materials; wherein, the silicon-rich raw materials are laid at the bottom of the reaction vessel, and the carbon-rich raw materials are filled on the surface of the silicon-rich raw materials, so that the silicon-rich raw materials are located in the lower layer of the reaction vessel and the silicon-rich raw materials are located in the upper layer of the reaction vessel.

[0027] The silicon-rich raw material includes silicon powder and carbon powder, and the molar amount of silicon in the silicon-rich raw material is greater than the molar amount of carbon; the carbon-rich raw material includes silicon powder and carbon powder, and the molar amount of carbon in the carbon-rich raw material is greater than the molar amount of silicon.

[0028] S02. Place the reaction vessel containing the raw material into a heating device, evacuate the heating device, and then heat it to cause the raw material to react and obtain silicon carbide.

[0029] The raw materials are divided into silicon-rich and carbon-rich materials and placed in layers, with the silicon-rich material in the lower layer and the carbon-rich material in the upper layer. After vacuuming, the material is heated. During heating, the excess carbon powder in the upper layer can react more fully with the silicon to form silicon carbide, significantly reducing the possibility of silicon vapor escaping from the material. Meanwhile, the sufficient silicon in the silicon-rich material in the lower layer can fully react with the carbon powder to form silicon carbide. After the reaction, the remaining silicon in the lower layer will sublimate into silicon vapor at high temperature. The silicon vapor diffuses upward and reacts with the remaining carbon powder in the upper layer to form silicon carbide. Compared with silicon particles, silicon vapor has a larger contact area with carbon powder, allowing the silicon element in the raw materials to react fully. This greatly reduces the risk of silicon vapor accumulating at the top of the reaction vessel and reacting with the vessel cover, as well as the risk of silicon vapor leakage. This significantly reduces the waste of raw materials and the wear and tear of the reaction vessel (e.g., crucible), thereby obtaining high-quality silicon carbide while significantly reducing the production cost of silicon carbide.

[0030] Furthermore, when the reaction vessel is equipped with insulation material (e.g., carbon fiber felt), the above preparation method can significantly reduce the risk of the insulation material being corroded by silicon vapor. The above preparation method is simple, highly controllable, and has high production efficiency, enabling large-scale industrial production.

[0031] In this application, the relative pressure mentioned above is equal to |absolute pressure - standard atmospheric pressure|.

[0032] In some embodiments of this application, the silicon powder is high-purity silicon powder, and the carbon powder is high-purity carbon powder.

[0033] In some embodiments of this application, the reaction vessel is a graphite crucible. In some specific embodiments, the inner wall of the graphite crucible is further provided with graphite paper to isolate the raw materials from the crucible and prevent silicon from reacting with carbon in the graphite crucible.

[0034] In some embodiments of this application, the reaction vessel is further provided with an insulating material. For example, the insulating material may be carbon fiber felt.

[0035] In some embodiments of this application, the heating device includes, but is not limited to, induction heating furnace, graphite resistance heating furnace, etc.

[0036] In some embodiments of this application, the molar ratio of carbon to silicon in the silicon-rich raw material is 1:(1.1-1.3). For example, the molar ratio of carbon to silicon in the silicon-rich raw material can be 1:1.1, 1:1.15, 1:1.2, 1:1.25, 1:1.3, etc. Thus, during the heating process, the silicon on the surface of the silicon particles first reacts with carbon to form silicon carbide. As the temperature rises further, the unreacted silicon (including the remaining silicon powder and the silicon inside the silicon powder particles wrapped by the generated silicon carbide) melts into an appropriate amount of molten silicon. This appropriate amount of molten silicon can be adhered to by the already generated silicon carbide or by the incompletely reacted carbon. At this point, the molten silicon can react with the aforementioned unreacted carbon to form silicon carbide. The remaining molten silicon can vaporize and diffuse to the upper layer as the temperature rises further, reacting with the remaining carbon powder in the upper layer. This appropriate amount of molten silicon will not accumulate at the bottom of the reaction vessel and corrode the vessel. It can also minimize the risk of excessive silicon vapor being generated, which would prevent the remaining carbon powder in the upper layer from reacting in time and cause a large amount of silicon vapor to accumulate and leak out at the top of the reaction vessel. This further reduces the risk of silicon vapor corroding the reaction vessel (e.g., crucible) and the insulation material (e.g., carbon fiber felt).

[0037] In some embodiments of this application, the molar ratio of silicon to carbon in the carbon-rich raw material is 1:(1.04-1.27). This ensures that excess carbon powder in the upper layer can fully react with the silicon powder, while sufficient carbon can react with silicon vapor diffused from the lower layer. This further reduces the risk of silicon vapor accumulation at the top of the reaction vessel and avoids waste of raw materials due to excess carbon powder. For example, the molar ratio of silicon to carbon in the carbon-rich raw material can be 1:1.04, 1:1.05, 1:1.06, 1:1.07, 1:1.08, 1:1.09, 1:1.0, 1:12, 1:15, 1:1.18, 1:1.20, 1:1.22, 1:1.23, 1:1.24, 1:1:25, 1:1.26, etc.

[0038] In some embodiments of this application, the molar ratio of silicon to carbon in the carbon-rich raw material is 1:(1.10-1.27). This minimizes the risk of silicon vapor accumulating at the top of the reaction vessel.

[0039] In some embodiments of this application, the mass percentage of the silicon-rich raw material is 30%-50% based on the total mass of the raw materials. That is, the mass of the silicon-rich raw material is 30%-50% of the total mass of the carbon-rich raw material and the silicon-rich raw material. For example, the mass of the silicon-rich raw material can be 30%, 35%, 40%, 45%, 50%, etc., of the total mass of the raw materials. In this way, an appropriate amount of carbon-rich raw material can have a suitable thickness, providing an upward channel of suitable length for silicon vapor diffused from the lower layer, so that the silicon vapor can react more fully with the carbon in the upper layer, further reducing the risk of silicon vapor accumulation at the top of the reaction vessel.

[0040] In some embodiments of this application, the molar ratio of carbon to silicon in the raw materials is 1:(1.00-1.05). Controlling the molar ratio of total silicon content to total carbon content in the raw materials to be close to 1 can result in higher quality silicon carbide. Exemplarily, the molar ratio of carbon to silicon in the raw materials is 1:1.00, 1:1.01, 1:1.02, 1:1.03, 1:1.04, 1:1.05, etc. In some specific embodiments, the molar ratio of carbon to silicon is 1:1. This ensures better purity and quality of the final silicon carbide product.

[0041] In some embodiments of this application, the heating includes:

[0042] S21. Evacuate the heating device until the relative pressure inside is less than or equal to 10. -5After mbar, the temperature is increased to 500℃-800℃ at a heating rate of 15℃ / min-20℃ / min; for example, the temperature can be increased to 500℃, 550℃, 600℃, 650℃, 700℃, 750℃, 775℃, etc. at heating rates of 15℃ / min, 16℃ / min, 17℃ / min, 18℃ / min, 19℃ / min, 20℃ / min, etc.

[0043] S22. Under the condition that the relative pressure inside the heating device is less than or equal to 10 mbar, continue to heat to 1300℃-1400℃ at a rate of 15℃ / min-20℃ / min. At this time, the heating rate can be maintained at the same rate as in S21, and the temperature can be raised to 1300℃, 1320℃, 1340℃, 1360℃, 1380℃, etc.; then introduce inert gas into the heating device until the relative pressure inside the heating device is 800mbar-1000mbar, while introducing the inert gas... The temperature is increased to a holding temperature of 2100℃-2400℃ at a second heating rate of 8℃ / min-10℃ / min, and held for 5h-10h to obtain silicon carbide. At this time, the relative pressure inside the heating device can be 800mbar, 850mbar, 900mbar, 950mbar, etc., and the temperature can be increased to the holding temperature at a second heating rate of 8℃ / min, 9℃ / min, 10℃ / min, etc. The holding temperature can be 2100℃, 2200℃, 2300℃, etc., and the holding time can be 5h, 6h, 7h, 8h, 9h, etc.

[0044] In S21, the vacuum is evacuated to 10. -5 mbar can initially remove adsorbed gases from the raw materials and prevent oxidation of the reaction vessel and any insulation materials during heating, thus promoting the reaction. In S22, some silicon reacts with carbon before the temperature reaches 1300℃-1400℃, but the silicon carbide formed at this time hinders the reaction between silicon and carbon inside the silicon particles in the raw materials. As the temperature rises to 1300℃-1400℃, unreacted silicon (including silicon inside the silicon particles) begins to melt, and SiC generated under high vacuum also begins to decompose. At this point, reducing the vacuum can suppress the decomposition of SiC inside the reaction vessel and the unnecessary volatilization of silicon and carbon raw materials. Simultaneously reducing the heating rate can slow down the temperature gradient inside the reaction vessel (the radial temperature gradient field from the center of the reaction vessel outward), thereby improving the uniformity of the particle size distribution of the final silicon carbide product. At the same time, it can more fully address the black core phenomenon caused by incomplete reaction of the raw materials in the center of the reaction vessel, improving the uniformity of the composition distribution of the final silicon carbide.

[0045] In some embodiments of this application, in step S21, at least one gas purging process is performed simultaneously with the heating. This gas purging process includes: introducing an inert gas into the heating device to a relative pressure of 500 mbar-800 mbar, maintaining this pressure for 10-15 minutes, and then evacuating the device until the relative pressure inside is less than or equal to 10 mbar. This removes the thermal field and further removes gases adsorbed in the raw materials, thereby improving the quality of the final silicon carbide product. In some specific embodiments, in step S21, two gas purging processes are performed simultaneously with the heating.

[0046] In some embodiments of this application, after step S22, the heating further includes step S23: evacuating the heating device to a relative pressure less than or equal to 30 mbar, then introducing inert gas again to a relative pressure of 500 mbar inside the heating device, and cooling down. This removes trace amounts of volatiles from the heating device (e.g., volatiles generated by the soft felt at high temperatures), preventing these traces from depositing on the inner wall of the heating device during cooling and from contaminating the product during cooling or removal of the silicon carbide.

[0047] The technical solution of this application is further described below with reference to several embodiments.

[0048] Example 1

[0049] (1) Two layers of graphite paper are laid on the inner wall of the graphite crucible and the raw materials (specifically, a mixture of high-purity carbon powder and high-purity silicon powder) are filled. First, 2.4 kg of silicon-rich raw material is loaded into the graphite crucible, and then 5.6 kg of carbon-rich raw material is loaded on the top layer of silicon-rich raw material. The molar ratio of carbon to silicon in the silicon-rich raw material is 1:1.10, and the molar ratio of silicon to carbon in the carbon-rich raw material is 1:1.04.

[0050] (2) Tighten the lid on the graphite crucible containing the above raw materials and place it in the heating device (specifically, an induction heating furnace). First, evacuate the furnace until the relative pressure inside the furnace is 10. -5 After reaching mbar, the gas is washed while heating at 15℃ / min: inert gas (specifically Ar) is introduced into the furnace until the relative pressure inside the furnace reaches 500 mbar and is maintained for 10 min. Then, the gas is evacuated until the relative pressure inside the furnace reaches 10 mbar. This process is repeated once. Then, the heating rate is kept constant and the temperature is continued to rise under the condition that the relative pressure inside the furnace is 10 mbar.

[0051] When the furnace temperature reaches 1300℃, an inert gas (specifically Ar) is introduced into the furnace, and the heating rate is reduced to 8℃ / min before continuing to heat to 2300℃ and holding for 5 hours.

[0052] After the heat preservation is completed, the furnace is evacuated again until the relative pressure inside the furnace reaches 30 mbar. Then, an inert gas (specifically Ar) is introduced into the furnace until the relative pressure inside the furnace reaches 500 mbar. The furnace is then cooled down until the temperature drops below 100°C, at which point the crucible is removed.

[0053] (3) The silicon carbide block in the crucible is crushed and sieved to obtain the final silicon carbide particles.

[0054] Example 2

[0055] The only difference from Example 1 is that the raw material composition in the graphite crucible is as follows: the lower layer is 4 kg of silicon-rich raw material, in which the molar ratio of carbon to silicon is 1:1.10, and the upper layer is 4 kg of carbon-rich raw material, in which the molar ratio of silicon to carbon is 1:1.10.

[0056] Example 3

[0057] The only difference from Example 1 is that the raw material composition in the graphite crucible is as follows: the lower layer is 2.4 kg of silicon-rich raw material, in which the molar ratio of carbon to silicon is 1:1.30, and the upper layer is 5.6 kg of carbon-rich raw material, in which the molar ratio of silicon to carbon is 1:1.11.

[0058] Example 4

[0059] The only difference from Example 1 is that the raw material composition in the graphite crucible is as follows: the lower layer is 4 kg of silicon-rich raw material, in which the molar ratio of carbon to silicon is 1:1.30, and the upper layer is 4 kg of carbon-rich raw material, in which the molar ratio of silicon to carbon is 1:1.27.

[0060] Example 5

[0061] The only difference from Example 1 is that the raw material composition in the graphite crucible is as follows: the lower layer is 4.8 kg of silicon-rich raw material, in which the molar ratio of carbon to silicon is 1:1.3, and the upper layer is 3.2 kg of carbon-rich raw material, in which the molar ratio of silicon to carbon is 1:1.42.

[0062] To highlight the beneficial effects of the embodiments of this application, the following comparative examples are provided.

[0063] Comparative Example 1

[0064] The difference from Example 1 is that in step (1) above, 8 kg of raw material is directly filled into a graphite crucible, wherein the raw material is a mixture of high-purity silicon and high-purity carbon, and the molar ratio of silicon to carbon in the raw material is 1:1.

[0065] After the silicon carbide prepared in the examples and comparative examples was removed, the same experiment was repeated four times for each example and comparative example using the same crucible. Before the first experiment for each example and comparative example, the thickness of each crucible lid was measured with a micrometer. After the fifth experiment, the thickness of each crucible lid was measured again with a micrometer. The difference between the two thickness measurements was regarded as the deposition thickness of the crucible lid. The greater the deposition thickness, the more severe the wear of the crucible lid. The results are summarized in Table 1.

[0066] Table 1

[0067]

[0068] As can be seen from the results in Table 1, the preparation of silicon carbide using the technical solution provided in this application can significantly reduce raw material waste and the wear of the reaction vessel (crucible). In addition, when the mass ratio of silicon-rich raw materials in the raw materials is within the preferred range of this application (Examples 1-4), the wear of the crucible is significantly smaller.

[0069] The above description is an exemplary embodiment of this application. It should be noted that those skilled in the art can make several improvements and modifications without departing from the principles of this application, and these improvements and modifications are also considered to be within the scope of protection of this application.

Claims

1. A method for preparing silicon carbide, characterized in that, The preparation method includes the following steps: (1) Loading raw materials into a reaction vessel, the raw materials including silicon-rich raw materials and carbon-rich raw materials; wherein, the silicon-rich raw materials are laid at the bottom of the reaction vessel, and the carbon-rich raw materials are filled on the surface of the silicon-rich raw materials, so that the silicon-rich raw materials are located in the lower layer of the reaction vessel, and the carbon-rich raw materials are located in the upper layer of the reaction vessel. The silicon-rich raw material includes silicon powder and carbon powder, and the molar amount of silicon in the silicon-rich raw material is greater than the molar amount of carbon; the carbon-rich raw material includes silicon powder and carbon powder, and the molar amount of carbon in the carbon-rich raw material is greater than the molar amount of silicon. (2) The reaction vessel containing the raw material is placed in a heating device, the heating device is evacuated, and then heated to obtain silicon carbide; wherein the heating includes: a) Evacuate the heating device until the relative pressure inside is less than or equal to 10. -5 After mbar, the temperature is increased to 500℃-800℃ at a heating rate of 15℃ / min-20℃ / min; b) Under the condition that the relative pressure inside the heating device is less than or equal to 10 mbar, the temperature is further increased to 1300-1400℃ at a rate of 15-20℃ / min. Inert gas is introduced into the heating device until the relative pressure inside the heating device is 800mbar-1000mbar. At the same time as the inert gas is introduced, the temperature is increased to 2100℃-2400℃ at a rate of 8℃ / min-10℃ / min and held for 5h-10h to obtain silicon carbide.

2. The preparation method according to claim 1, characterized in that, In the silicon-rich raw material, the molar ratio of carbon to silicon is 1:(1.1-1.3).

3. The preparation method according to claim 1, characterized in that, In the carbon-rich raw material, the molar ratio of silicon to carbon is 1:(1.04-1.27).

4. The preparation method according to claim 3, characterized in that, In the carbon-rich raw material, the molar ratio of silicon to carbon is 1:(1.10-1.27).

5. The preparation method according to claim 1, characterized in that, Based on the total mass of the raw materials, the mass percentage of the silicon-rich raw materials is 30%-50%.

6. The preparation method according to any one of claims 1-5, characterized in that, In the raw materials, the molar ratio of carbon to silicon is 1:

1.

7. The preparation method according to any one of claims 1-5, characterized in that, The reaction vessel is a graphite crucible; wherein, the inner wall of the graphite crucible is also lined with graphite paper.

8. The preparation method according to any one of claims 1-5, characterized in that, After step b), the heating further includes: evacuating the heating device to a relative pressure of less than or equal to 30 mbar, then introducing inert gas again to a relative pressure of 500 mbar-800 mbar inside the heating device, and cooling it down.

9. The preparation method according to claim 1, characterized in that, In step a), at least one gas scrubbing process is performed simultaneously with the heating, the gas scrubbing process including: Inert gas is introduced into the heating device until the relative pressure inside the heating device is 500mbar-800mbar, and the pressure is maintained for 10min-15min. Then, a vacuum is drawn until the relative pressure inside the heating device is less than or equal to 10mbar.

Citation Information

Patent Citations

  • Method for improving growth rate of silicon carbide ceramic

    CN112939605A