Corrosion-resistant high-strength aluminum-magnesium alloy welding wire and preparation process thereof

Aluminum-magnesium alloy welding wire was prepared by ball milling and mixing modified nanofillers with copper powder, which solved the problem of poor dispersion of reinforcing materials and achieved a high-strength and corrosion-resistant aluminum-magnesium alloy welding wire.

CN118492748BActive Publication Date: 2026-11-24JIANGSU GANGCANG NEW MATERIAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410728240.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-06
Publication Date
2026-11-24
Estimated Expiration
2044-06-06

AI Technical Summary

Technical Problem

The existing aluminum-magnesium alloy welding wires exhibit poor dispersibility after the addition of reinforcing materials, resulting in reduced strength and corrosion resistance.

Method used

The process involves modifying the material with nanofillers, including graphene oxide sheets and boron nitride nanotubes, improving dispersibility with modifiers, and mixing it with copper powder through ball milling. This is followed by the addition of aluminum ingots, magnesium ingots, and other alloys for smelting to form a composite material, thus optimizing the welding wire preparation process.

Benefits of technology

It improves the strength and corrosion resistance of aluminum-magnesium alloy welding wire, forms a uniform network structure, prevents copper migration, and enhances the mechanical properties and corrosion resistance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004879377330000081
    Figure BDA0004879377330000081
Patent Text Reader

Abstract

This invention relates to the field of alloy welding wire technology, specifically to a corrosion-resistant, high-strength aluminum-magnesium alloy welding wire and its preparation process. The process includes the following steps: Step 1: Placing nanofillers in a copper solution containing a modifier for modification treatment; obtaining modified nanofillers; Step 2: Ball milling and mixing the modified nanofillers with copper powder to obtain a composite material; Step 3: Melting aluminum ingots, magnesium ingots, aluminum-chromium master alloy, zinc ingots, and aluminum-silicon master alloy; adding the composite material, homogenizing, casting, drawing, and post-processing to obtain the aluminum-magnesium alloy welding wire. Beneficial effects: The addition of graphene sheets and boron nitride nanotubes to the aluminum-magnesium alloy welding wire enhances its strength and corrosion resistance through a synergistic effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of alloy welding wire technology, specifically to a corrosion-resistant, high-strength aluminum-magnesium alloy welding wire and its preparation process. Background Technology

[0002] Aluminum-magnesium alloy welding wire is a filler material specifically designed for welding aluminum alloys. Due to its excellent welding process performance and the mechanical properties of the weld metal, this type of wire is widely used in welding aluminum alloy structures, especially in applications requiring high strength, crack resistance, and corrosion resistance. The use of aluminum-magnesium alloy welding wire can significantly improve the quality of welded joints, meeting the high standards required for aluminum alloy welding in industries such as aerospace, automotive, and shipbuilding. With the increasing prevalence of aluminum alloy materials in lightweight and high-performance applications, the importance of aluminum-magnesium alloy welding wire is becoming increasingly prominent.

[0003] In existing technologies, reinforcing materials such as graphene sheets are typically added to improve the strength and corrosion resistance of aluminum-magnesium alloy welding wires. However, the dispersion of these reinforcing materials in the alloy is poor, and they are prone to aggregation, leading to reduced strength and density, and poor corrosion resistance. Therefore, to address these issues, a corrosion-resistant, high-strength aluminum-magnesium alloy welding wire has been developed. Summary of the Invention

[0004] The purpose of this invention is to provide a corrosion-resistant, high-strength aluminum-magnesium alloy welding wire and its preparation process, so as to solve the problems mentioned in the background art.

[0005] To solve the above-mentioned technical problems, the present invention provides the following technical solution:

[0006] A process for preparing a corrosion-resistant, high-strength aluminum-magnesium alloy welding wire includes the following steps:

[0007] Step 1: Place the nanofiller in a copper solution containing a modifier for modification treatment; obtain the modified nanofiller.

[0008] Step 2: The modified nanofiller and copper powder are ball-milled and mixed to obtain the composite material;

[0009] Step 3: Melt aluminum ingots, magnesium ingots, aluminum-chromium master alloy, zinc ingots, and aluminum-silicon master alloy; add composite materials, homogenize, cast ingots, draw into shape, and perform post-treatment to obtain aluminum-magnesium alloy welding wire.

[0010] In a more optimized manner, the nanofiller comprises graphene oxide sheets and boron nitride nanotubes in a mass ratio of 1:(1.2-1.5).

[0011] In a more optimized manner, the copper solution comprises the following raw materials: 7-8 g / L NaOH, 5-7 g / L anhydrous copper sulfate, 12-15 mL formaldehyde, 25-30 g / L potassium sodium tartrate, and 1-2 g / L modifier; the amount of nanofiller added is 0.8-1.2 wt% of the copper solution.

[0012] In a more optimized manner, the raw materials of the composite material include modified nanofillers and copper powder in a mass ratio of (2-4):(10-12).

[0013] More optimally, the raw materials of the aluminum-magnesium alloy welding wire include the following components: by weight, 10-12 parts aluminum ingot, 0.5-0.8 parts magnesium ingot, 0.1-0.2 parts aluminum-chromium master alloy, 0.1-0.2 parts zinc ingot, 0.2-0.3 parts aluminum-silicon master alloy, and 0.1-0.2 parts composite material.

[0014] A more optimized approach is to use the following process parameters for modification: set an electrostatic field with a frequency of 70–80 kV / m, and perform modification treatment at a temperature of 70–80 °C for 60–80 min.

[0015] In a more optimized manner, the specific process of ball milling and mixing is as follows: the modified nanofiller and copper powder are loaded into a ball mill jar containing steel balls, and 150-200 mL of anhydrous ethanol is added. The rotation speed of the ball mill is set to 300-500 r / min, and ball milling is carried out for 3-5 hours to obtain the composite material. The process parameters of the melting are: temperature 750-780℃, time 10-12 hours; the ingot temperature is 680-700℃; the wire diameter of the drawn wire is 6-8 mm; the process parameters of the post-treatment are: solution temperature 520-560℃, time 80-90 min; aging temperature 320-380℃, aging time 1-2 hours, with both solution treatment and aging carried out in a high-purity argon atmosphere at a gas flow rate of 25-30 L / min.

[0016] In a more optimized manner, the preparation process of the modifier is as follows: (1) Mix hexyl magnesium bromide, 1,3-bis(diphenylphosphine) nickel dichloride and o-dichlorobenzene and react for 6-8 h, and separate to obtain intermediate A; (2) Mix intermediate A, maleic anhydride and carbon disulfide and stir, add anhydrous AlCl3 in batches, react for 30-50 min, and separate to obtain intermediate B; (3) Dissolve intermediate B in ethanol, adjust the pH to 7-8 with sodium hydroxide aqueous solution, distill under reduced pressure, and dry to obtain the modifier.

[0017] More optimally, intermediate A comprises the following components: by mass parts, 1-2 parts of hexyl magnesium bromide, 0.2-0.5 parts of 1,3-bis(diphenylphosphine propane) nickel dichloride, and 0.8-1 parts of o-dichlorobenzene; intermediate B comprises the following components: by mass parts, 1-2 parts of intermediate A, 2-3 parts of maleic anhydride, 0.2-0.3 parts of carbon disulfide, and 0.5-0.7 parts of AlCl3.

[0018] This invention incorporates two-dimensional graphene sheets and one-dimensional boron nitride nanotubes into aluminum-magnesium alloy welding wire. The synergistic effect of these two materials enhances the strength and corrosion resistance of the welding wire. Simultaneously, to improve dispersion, a modifier containing a large number of hydrophilic groups is prepared. Details are as follows:

[0019] Firstly, a composite material containing graphene oxide sheets and boron nitride nanotubes is added to an aluminum-magnesium alloy and smelted together. The addition of copper will precipitate the CuAl2 phase during aging, which has a significant aging strengthening effect. However, copper will diffuse in certain environments, reducing the corrosion resistance of the material. The graphene sheets and boron nitride nanotubes added in this invention are well dispersed in the material, which can effectively prevent the migration of copper.

[0020] Secondly, graphene sheets and boron nitride nanotubes in aluminum-magnesium alloy welding wire can form a three-dimensional network structure, which plays a role in transmitting force when the aluminum-magnesium alloy welding wire is subjected to force, so that the material can be uniformly stressed and enhance the mechanical properties of the material. Graphene sheets and boron nitride nanotubes have strong stability and can enhance the corrosion resistance of the material. At the same time, the one-dimensional boron nitride nanotubes can restrain the aggregation of two-dimensional graphene sheets. The boron nitride nanotubes can be embedded in the layers of graphene sheets, preventing the aggregation between graphene sheets, and further enhancing the strength and corrosion resistance of the welding wire.

[0021] Thirdly, the interfacial wettability between graphene sheets and boron nitride nanotubes and copper is poor. The modifier synthesized in this invention has a longer molecular chain, which enhances the dispersibility of graphene sheets and boron nitride nanotubes. At the same time, as an anionic surfactant, it can perform better in alkaline copper solutions. Its hydrophilic groups can effectively improve the wettability of the material, enhance the adsorption effect of copper ions, and increase the dispersibility of graphene sheets and nano-boron nitride in aluminum-magnesium alloy welding wire. Detailed Implementation

[0022] The technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0023] It should be noted that the following parts are by weight. There are no special restrictions on the manufacturers of the raw materials involved in this invention. Exemplary examples include: graphene oxide sheets with a thickness ≤ 5 nm and a layer count < 5, purchased from Xianfeng Nano; boron nitride nanotube sheets with a diameter of 1–5 μm, a thickness < 5 nm, and a CAS value of 7440–42–8, purchased from Xianfeng Nano; hexyl magnesium bromide with a CAS value of 3761–92–0, purchased from Jacks; 1,3–bis(diphenylphosphine propane) nickel dichloride with a CAS value of 15629–92–2, purchased from Jusheng; aluminum ingots are ZL101; aluminum-chromium master alloy is AlCr2; aluminum-silicon master alloy is AlSi. 20 The zinc ingots have a purity of 4N to 7N and were purchased from Xinkang.

[0024] Example 1: A preparation process for a corrosion-resistant, high-strength aluminum-magnesium alloy welding wire, comprising the following steps:

[0025] Pre-preparation: Synthesis of the modifier: (1) Mix 1 part hexyl magnesium bromide, 0.2 parts 1,3-bis(diphenylphosphine) nickel dichloride, and 0.8 parts o-dichlorobenzene and react for 6-8 h, then separate to obtain intermediate A; (2) Mix 1 part intermediate A, 2 parts maleic anhydride, and 0.2 parts carbon disulfide and stir, then add 0.5 parts anhydrous AlCl3 in batches, react for 30 min, and allow to stand for separation. Remove the aqueous phase, take the organic phase, evaporate the solvent, and dry under vacuum to obtain intermediate B; (3) Dissolve intermediate B in ethanol, adjust the pH to 7 using 10% sodium hydroxide aqueous solution, stir at room temperature for 1 h, remove the solvent by vacuum distillation, and dry to obtain the modifier.

[0026] Pre-preparation: Preparation of boron nitride nanotubes: Boron nitride nanotubes were mixed with water and subjected to magnetic stirring and ultrasonic treatment. Bromine water was then added to the water mixture until the mixture turned orange-red, indicating the end of the functionalization process. The mixture was filtered, washed with water, and dried to obtain boron nitride nanotubes.

[0027] Step 1: Place 1 part graphene oxide sheet and 1.2 parts boron nitride nanotubes in a copper solution containing a modifier, and modify them at 70℃ for 60 min under an electrostatic field of 70 kV / m to obtain modified nanofiller;

[0028] Step 2: 2 parts of modified nanofiller and 10 parts of copper powder were placed into a ball mill jar containing steel balls, and 150 mL of anhydrous ethanol was added. The rotation speed of the ball mill was set to 300 r / min, and the mixture was ball milled for 3 h. After separation and drying, the composite material was obtained.

[0029] Step 3: Melt 10 parts aluminum ingot, 0.5 parts magnesium ingot, 0.1 parts aluminum-chromium master alloy, 0.1 parts zinc ingot, 0.2 parts aluminum-silicon master alloy, and 0.1 parts composite material at 750℃ for 10 hours, cool to 680℃ to cast ingot, then draw the wire diameter to 6mm, and perform solidification at 520℃ for 80 minutes under high-purity argon gas, followed by aging at 320℃ for 1 hour to finally obtain aluminum-magnesium alloy welding wire.

[0030] Example 2: A preparation process for a corrosion-resistant, high-strength aluminum-magnesium alloy welding wire, comprising the following steps:

[0031] Pre-preparation: Synthesis of the modifier: (1) Mix 1 part hexyl magnesium bromide, 0.2 parts 1,3-bis(diphenylphosphine) nickel dichloride, and 0.8 parts o-dichlorobenzene and react for 6-8 h, then separate to obtain intermediate A; (2) Mix 1 part intermediate A, 2 parts maleic anhydride, and 0.2 parts carbon disulfide and stir, then add 0.5 parts anhydrous AlCl3 in batches, react for 30 min, and allow to stand for separation. Remove the aqueous phase, take the organic phase, evaporate the solvent, and dry under vacuum to obtain intermediate B; (3) Dissolve intermediate B in ethanol, adjust the pH to 7 using 10% sodium hydroxide aqueous solution, stir at room temperature for 1 h, remove the solvent by vacuum distillation, and dry to obtain the modifier.

[0032] Pre-preparation: Preparation of boron nitride nanotubes: Boron nitride nanotubes were mixed with water and subjected to magnetic stirring and ultrasonic treatment. Bromine water was then added to the water mixture until the mixture turned orange-red, indicating the end of the functionalization process. The mixture was filtered, washed with water, and dried to obtain boron nitride nanotubes.

[0033] Step 1: Place 1 part graphene oxide sheet and 1.5 parts boron nitride nanotubes in a copper solution containing a modifier, and modify them at 80℃ for 80 min under an electrostatic field of 80 kV / m to obtain modified nanofiller.

[0034] Step 2: 4 parts of modified nanofiller and 12 parts of copper powder were loaded into a ball mill jar containing steel balls, and 200 mL of anhydrous ethanol was added. The rotation speed of the ball mill was set to 500 r / min, and the mixture was ball milled for 5 h. After separation and drying, the composite material was obtained.

[0035] Step 3: Melt 12 parts aluminum ingot, 0.8 parts magnesium ingot, 0.2 parts aluminum-chromium master alloy, 0.2 parts zinc ingot, 0.3 parts aluminum-silicon master alloy, and 0.2 parts composite material at 780℃ for 12 hours, cool to 700℃ to cast ingot, then draw the wire diameter to 8mm, and perform solidification at 560℃ for 90 minutes under high-purity argon gas, followed by aging at 380℃ for 2 hours to finally obtain aluminum-magnesium alloy welding wire.

[0036] Example 3: A preparation process for a corrosion-resistant, high-strength aluminum-magnesium alloy welding wire, comprising the following steps:

[0037] Pre-preparation: Synthesis of the modifier: (1) Mix 1 part hexyl magnesium bromide, 0.2 parts 1,3-bis(diphenylphosphine) nickel dichloride, and 0.8 parts o-dichlorobenzene and react for 6-8 h, then separate to obtain intermediate A; (2) Mix 1 part intermediate A, 2 parts maleic anhydride, and 0.2 parts carbon disulfide and stir, then add 0.5 parts anhydrous AlCl3 in batches, react for 30 min, and allow to stand for separation. Remove the aqueous phase, take the organic phase, evaporate the solvent, and dry under vacuum to obtain intermediate B; (3) Dissolve intermediate B in ethanol, adjust the pH to 7 using 10% sodium hydroxide aqueous solution, stir at room temperature for 1 h, remove the solvent by vacuum distillation, and dry to obtain the modifier.

[0038] Pre-preparation: Preparation of boron nitride nanotubes: Boron nitride nanotubes were mixed with water and subjected to magnetic stirring and ultrasonic treatment. Bromine water was then added to the water mixture until the mixture turned orange-red, indicating the end of the functionalization process. The mixture was filtered, washed with water, and dried to obtain boron nitride nanotubes.

[0039] Step 1: Place 1 part graphene oxide sheet and 1.5 parts boron nitride nanotubes in a copper solution containing a modifier, and modify them at 75℃ for 70 min under an electrostatic field of 75kV / m to obtain modified nanofiller.

[0040] Step 2: 3 parts of modified nanofiller and 11 parts of copper powder were loaded into a ball mill jar containing steel balls, and 160 mL of anhydrous ethanol was added. The rotation speed of the ball mill was set to 400 r / min, and the mixture was ball milled for 4 h. After separation and drying, the composite material was obtained.

[0041] Step 3: Melt 10 parts aluminum ingot, 0.5 parts magnesium ingot, 0.1 parts aluminum-chromium master alloy, 0.1 parts zinc ingot, 0.2 parts aluminum-silicon master alloy, and 0.1 parts composite material at 750℃ for 10 hours, cool to 680℃ to cast ingot, then draw the wire diameter to 6mm, and perform solidification at 520℃ for 80 minutes under high-purity argon gas, followed by aging at 320℃ for 1 hour to finally obtain aluminum-magnesium alloy welding wire.

[0042] Example 4: A preparation process for a corrosion-resistant, high-strength aluminum-magnesium alloy welding wire, comprising the following steps:

[0043] Pre-preparation: Synthesis of the modifier: (1) Mix 1 part hexyl magnesium bromide, 0.2 parts 1,3-bis(diphenylphosphine) nickel dichloride, and 0.8 parts o-dichlorobenzene and react for 6-8 h, then separate to obtain intermediate A; (2) Mix 1 part intermediate A, 2 parts maleic anhydride, and 0.2 parts carbon disulfide and stir, then add 0.5 parts anhydrous AlCl3 in batches, react for 30 min, and allow to stand for separation. Remove the aqueous phase, take the organic phase, evaporate the solvent, and dry under vacuum to obtain intermediate B; (3) Dissolve intermediate B in ethanol, adjust the pH to 7 using 10% sodium hydroxide aqueous solution, stir at room temperature for 1 h, remove the solvent by vacuum distillation, and dry to obtain the modifier.

[0044] Pre-preparation: Preparation of boron nitride nanotubes: Boron nitride nanotubes were mixed with water and subjected to magnetic stirring and ultrasonic treatment. Bromine water was then added to the water mixture until the mixture turned orange-red, indicating the end of the functionalization process. The mixture was filtered, washed with water, and dried to obtain boron nitride nanotubes.

[0045] Step 1: Place 1 part graphene oxide sheet and 1.5 parts boron nitride nanotubes in a copper solution containing a modifier, and modify them at 75℃ for 70 min under an electrostatic field of 75kV / m to obtain modified nanofiller.

[0046] Step 2: 3 parts of modified nanofiller and 11 parts of copper powder were loaded into a ball mill jar containing steel balls, and 160 mL of anhydrous ethanol was added. The rotation speed of the ball mill was set to 400 r / min, and the mixture was ball milled for 4 h. After separation and drying, the composite material was obtained.

[0047] Step 3: Melt 11 parts aluminum ingot, 0.6 parts magnesium ingot, 0.15 parts aluminum-chromium master alloy, 0.15 parts zinc ingot, 0.25 parts aluminum-silicon master alloy, and 0.15 parts composite material at 760℃ for 11 hours, cool to 690℃ to cast ingot, then draw the wire diameter to 7mm, and perform solidification at 540℃ for 85 minutes under high-purity argon gas, followed by aging at 360℃ for 1.5 hours to finally obtain aluminum-magnesium alloy welding wire.

[0048] Comparative Example 1: No hydroxyl-containing boron nanoparticles were added; all other aspects were the same as in Example 3, as detailed below:

[0049] Pre-preparation: Synthesis of the modifier: (1) Mix 1 part hexyl magnesium bromide, 0.2 parts 1,3-bis(diphenylphosphine) nickel dichloride, and 0.8 parts o-dichlorobenzene and react for 6-8 h, then separate to obtain intermediate A; (2) Mix 1 part intermediate A, 2 parts maleic anhydride, and 0.2 parts carbon disulfide and stir, then add 0.5 parts anhydrous AlCl3 in batches, react for 30 min, and allow to stand for separation. Remove the aqueous phase, take the organic phase, evaporate the solvent, and dry under vacuum to obtain intermediate B; (3) Dissolve intermediate B in ethanol, adjust the pH to 7 using 10% sodium hydroxide aqueous solution, stir at room temperature for 1 h, remove the solvent by vacuum distillation, and dry to obtain the modifier.

[0050] Step 1: Place one part of graphene oxide sheet in a copper solution containing a modifier, and modify it at 75℃ for 70 min under an electrostatic field of 75kV / m to obtain modified nanofiller.

[0051] Step 2: 3 parts of modified nanofiller and 11 parts of copper powder were loaded into a ball mill jar containing steel balls, and 160 mL of anhydrous ethanol was added. The rotation speed of the ball mill was set to 400 r / min, and the mixture was ball milled for 4 h. After separation and drying, the composite material was obtained.

[0052] Step 3: Melt 11 parts aluminum ingot, 0.6 parts magnesium ingot, 0.15 parts aluminum-chromium master alloy, 0.15 parts zinc ingot, 0.25 parts aluminum-silicon master alloy, and 0.15 parts composite material at 760℃ for 11 hours, cool to 690℃ to cast ingot, then draw the wire diameter to 7mm, and perform solidification at 540℃ for 85 minutes under high-purity argon gas, followed by aging at 360℃ for 1.5 hours to finally obtain aluminum-magnesium alloy welding wire.

[0053] Comparative Example 2: An excess of graphene sheets was added, and the rest was the same as in Example 3, as follows:

[0054] Pre-preparation: Synthesis of the modifier: (1) Mix 1 part hexyl magnesium bromide, 0.2 parts 1,3-bis(diphenylphosphine) nickel dichloride, and 0.8 parts o-dichlorobenzene and react for 6-8 h, then separate to obtain intermediate A; (2) Mix 1 part intermediate A, 2 parts maleic anhydride, and 0.2 parts carbon disulfide and stir, then add 0.5 parts anhydrous AlCl3 in batches, react for 30 min, and allow to stand for separation. Remove the aqueous phase, take the organic phase, evaporate the solvent, and dry under vacuum to obtain intermediate B; (3) Dissolve intermediate B in ethanol, adjust the pH to 7 using 10% sodium hydroxide aqueous solution, stir at room temperature for 1 h, remove the solvent by vacuum distillation, and dry to obtain the modifier.

[0055] Pre-preparation: Preparation of boron nitride nanotubes: Boron nitride nanotubes were mixed with water and subjected to magnetic stirring and ultrasonic treatment. Bromine water was then added to the water mixture until the mixture turned orange-red, indicating the end of the functionalization process. The mixture was filtered, washed with water, and dried to obtain boron nitride nanotubes.

[0056] Step 1: Place 8 parts of graphene oxide sheets and 1.5 parts of boron nitride nanotubes in a copper solution containing a modifier, and modify them at 75℃ for 70 min under an electrostatic field of 75kV / m to obtain modified nanofillers.

[0057] Step 2: 3 parts of modified nanofiller and 11 parts of copper powder were loaded into a ball mill jar containing steel balls, and 160 mL of anhydrous ethanol was added. The rotation speed of the ball mill was set to 400 r / min, and the mixture was ball milled for 4 h. After separation and drying, the composite material was obtained.

[0058] Step 3: Melt 11 parts aluminum ingot, 0.6 parts magnesium ingot, 0.15 parts aluminum-chromium master alloy, 0.15 parts zinc ingot, 0.25 parts aluminum-silicon master alloy, and 0.15 parts composite material at 760℃ for 11 hours, cool to 690℃ to cast ingot, then draw the wire diameter to 7mm, and perform solidification at 540℃ for 85 minutes under high-purity argon gas, followed by aging at 360℃ for 1.5 hours to finally obtain aluminum-magnesium alloy welding wire.

[0059] Comparative Example 3: No modifier was added to the copper solution, and everything else was the same as in Example 3, as follows:

[0060] Pre-preparation: Preparation of boron nitride nanotubes: Boron nitride nanotubes were mixed with water and subjected to magnetic stirring and ultrasonic treatment. Bromine water was then added to the water mixture until the mixture turned orange-red, indicating the end of the functionalization process. The mixture was filtered, washed with water, and dried to obtain boron nitride nanotubes.

[0061] Step 1: Place 1 part of graphene oxide sheet and 1.5 parts of boron nitride nanotubes in a copper solution and modify them at 75℃ for 70 min with an electrostatic field of 75kV / m to obtain nanofiller;

[0062] Step 2: Place 3 parts of nanofiller and 11 parts of copper powder into a ball mill jar containing steel balls, add 160 mL of anhydrous ethanol, set the rotation speed of the ball mill to 400 r / min, ball mill for 4 h, separate and dry to obtain the composite material;

[0063] Step 3: Melt 11 parts aluminum ingot, 0.6 parts magnesium ingot, 0.15 parts aluminum-chromium master alloy, 0.15 parts zinc ingot, 0.25 parts aluminum-silicon master alloy, and 0.15 parts composite material at 760℃ for 11 hours, cool to 690℃ to cast ingot, then draw the wire diameter to 7mm, and perform solidification at 540℃ for 85 minutes under high-purity argon gas, followed by aging at 360℃ for 1.5 hours to finally obtain aluminum-magnesium alloy welding wire.

[0064] Comparative Example 4: Commonly available aluminum-magnesium alloy welding wire was used.

[0065] Testing experiments: The tensile strength of the aluminum-magnesium alloy welding wires prepared in the examples and comparative examples was tested at 25°C and a rate of 1 mm / min. Corrosion resistance testing was conducted in a SWAAT salt spray chamber, with a 12-hour cycle per day. Each cycle consisted of 30 minutes of salt spray followed by 90 minutes of 50°C condensate humidification. The corrosion depth was tested after 60 days. The measured data are shown in the table below:

[0066]

[0067] Table 1

[0068] Conclusion: The aluminum-magnesium alloy welding wires prepared in Examples 1-4, by incorporating two-dimensional graphene sheets and one-dimensional boron nitride nanotubes, exhibited a synergistic effect, effectively enhancing the strength and corrosion resistance of the welding wire compared to Comparative Example 4. In Comparative Example 1, without the addition of nano-boron nitride, the graphene sheets agglomerated, resulting in overlapping layers and loss of good guidance. Simultaneously, the lack of reinforcing material, boron nitride nanotubes, reduced the strength of the welding wire, leading to a performance decrease compared to the optimal example 4. In Comparative Example 2, the addition of excessive graphene sheets disrupted the balance between graphene sheets and boron nitride nanotubes, causing strong agglomeration of both, resulting in a performance decrease compared to the optimal example 4. In Comparative Example 3, the nanofiller was not modified, resulting in poor dispersion of the nanofiller in the aluminum-magnesium alloy welding wire, leading to a performance decrease compared to the optimal example 4.

[0069] In the description of this specification, the references to terms such as "an embodiment," "example," "specific example," etc., indicate that a specific feature, structure, material, or characteristic described in connection with that embodiment or example is included in at least one embodiment or example of the present invention. In this specification, the illustrative expressions of the above terms do not necessarily refer to the same embodiment or example. Furthermore, the specific features, structures, materials, or characteristics described may be combined in any suitable manner in one or more embodiments or examples.

[0070] Finally, it should be noted that the above descriptions are merely preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the foregoing embodiments, those skilled in the art can still modify the technical solutions described in the foregoing embodiments or make equivalent substitutions for some of the technical features. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A preparation process for a corrosion-resistant, high-strength aluminum-magnesium alloy welding wire, characterized in that: Includes the following steps: Step 1: Place the nanofiller in a copper solution containing a modifier, set an electrostatic field with a frequency of 70~80kV / m, and modify it at a temperature of 70~80℃ for 60~80min; thus obtaining the modified nanofiller. Step 2: The modified nanofiller and copper powder are ball-milled and mixed to obtain the composite material; Step 3: Melt aluminum ingots, magnesium ingots, aluminum-chromium master alloy, zinc ingots, and aluminum-silicon master alloy; add composite materials, homogenize, cast ingots, draw into shape, and perform post-processing to obtain aluminum-magnesium alloy welding wire; The nanofiller comprises graphene oxide sheets and boron nitride nanotubes in a mass ratio of 1:(1.2~1.5); The preparation process of the modifier is as follows: (1) Mix hexyl magnesium bromide, 1,3-bis(diphenylphosphine) nickel dichloride and o-dichlorobenzene and react for 6-8 h, and separate to obtain intermediate A; (2) Mix intermediate A, maleic anhydride and carbon disulfide and stir, add anhydrous AlCl3 in batches, react for 30-0 min, and separate to obtain intermediate B; (3) Dissolve intermediate B in ethanol, adjust pH to 7-8 with sodium hydroxide aqueous solution, distill under reduced pressure and dry to obtain the modifier.

2. The preparation process of a corrosion-resistant high-strength aluminum-magnesium alloy welding wire according to claim 1, characterized in that: The copper solution comprises the following raw materials: 7~8 g / L NaOH, 5~7 g / L anhydrous copper sulfate, 12~15 mL formaldehyde, 25~30 g / L potassium sodium tartrate, and 1~2 g / L modifier; the amount of nanofiller added is 0.8~1.2 wt% of the copper solution.

3. The preparation process of a corrosion-resistant high-strength aluminum-magnesium alloy welding wire according to claim 1, characterized in that: The raw materials for the composite material include modified nanofillers and copper powder in a mass ratio of (2~4):(10~12).

4. The preparation process of a corrosion-resistant high-strength aluminum-magnesium alloy welding wire according to claim 1, characterized in that: The raw materials of the aluminum-magnesium alloy welding wire include the following components by weight: 10-12 parts aluminum ingot, 0.5-0.8 parts magnesium ingot, 0.1-0.2 parts aluminum-chromium master alloy, 0.1-0.2 parts zinc ingot, 0.2-0.3 parts aluminum-silicon master alloy, and 0.1-0.2 parts composite material.

5. The preparation process of a corrosion-resistant high-strength aluminum-magnesium alloy welding wire according to claim 1, characterized in that: The specific process of ball milling is as follows: modified nanofiller and copper powder are loaded into a ball mill jar containing steel balls, and 150-200 mL of anhydrous ethanol is added. The rotation speed of the ball mill is set to 300-500 r / min, and the ball milling is carried out for 3-5 hours to obtain the composite material. The process parameters of the melting are: temperature 750-780℃, time 10-12 hours; ingot temperature 680-700℃; wire diameter of the drawn wire is 6-8 mm; the process parameters of the post-treatment are: solution temperature 520-560℃, time 80-90 min; aging temperature 320-380℃, aging time 1-2 hours. Both solution treatment and aging are carried out in a high-purity argon atmosphere with a gas flow rate of 25-30 L / min.

6. The preparation process of a corrosion-resistant high-strength aluminum-magnesium alloy welding wire according to claim 1, characterized in that: Intermediate A comprises the following components: by mass, 1-2 parts of hexyl magnesium bromide, 0.2-0.5 parts of 1,3-bis(diphenylphosphine propane) nickel dichloride, and 0.8-1 parts of o-dichlorobenzene; Intermediate B comprises the following components: by mass, 1-2 parts of intermediate A, 2-3 parts of maleic anhydride, 0.2-0.3 parts of carbon disulfide, and 0.5-0.7 parts of AlCl3.

7. The corrosion-resistant high-strength aluminum-magnesium alloy welding wire obtained by the preparation process of the corrosion-resistant high-strength aluminum-magnesium alloy welding wire according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Processing process of corrosion-resistant aluminum-magnesium alloy

    CN109706335A

  • Design and preparation method of reinforced aluminum alloy corrosion-resistant welding wire based on doped nanowires

    CN117862738A