Supporting plate for firing

By setting an oxide first layer containing Zr, Si and Y elements and a yttrium oxide layer on the surface of the substrate of the firing support plate, the problem of substrate component penetration caused by coating peeling is solved, and the durability and service life of the firing support plate are improved.

CN118510739BActive Publication Date: 2026-11-24NGK INSULATORS LTD +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202280087686.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-03-28
Filing Date
2022-08-26
Publication Date
2026-11-24
Estimated Expiration
2042-08-26

AI Technical Summary

Technical Problem

When the coating of the existing firing plate is peeled off, the substrate components move into the object being fired, causing a reaction that damages the function of the firing plate and affects its durability.

Method used

An oxide first layer containing Zr, Si and Y elements is formed on the surface of the substrate, and a yttrium oxide layer is formed on it to improve the adhesion between coatings and inhibit the penetration of substrate components.

Benefits of technology

By improving the adhesion between coatings, the durability of the firing plate used for firing is enhanced, the penetration of components of the fired material is prevented, and the service life is extended.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118510739B_ABST
    Figure CN118510739B_ABST
Patent Text Reader

Abstract

The firing plate for firing has: a mullite layer, a first layer disposed on the mullite layer and being an oxide containing Zr, Si and Y elements, and a yttrium oxide layer disposed on the first layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application claims priority to Japanese Patent Application No. 2022-051967, filed March 28, 2022. The entire contents of that application are incorporated herein by reference. This specification discloses technology related to firing plates for firing. Background Technology

[0002] Japanese Patent Application Publication No. 2002-154884 (hereinafter referred to as Patent Document 1) discloses a firing plate for firing with a coating on the surface of a substrate. The coating is provided to suppress the reaction between the work to be fired and the substrate. In Patent Document 1, in order to reliably suppress the reaction between the work to be fired and the substrate, two or more coatings of different materials are provided on the surface of the substrate. In Patent Document 1, a coating is formed by providing two or more sprayed layers, or by providing a spray-plated layer on the surface of the sprayed layer. Summary of the Invention

[0003] The problem that the invention aims to solve

[0004] As in Patent Document 1, by providing two or more coating layers on the surface of the substrate, the reaction between the workpiece and the substrate can be suppressed, allowing for efficient firing of the workpiece. However, if a portion of the coating peels off (peeling occurs between the coating layers), components contained in the substrate will migrate to the workpiece, causing a reaction between the workpiece and the substrate components. In other words, if a portion of the coating peels off, its function as a firing support plate for firing is impaired. Therefore, when two or more coating layers are provided on the surface of the substrate, sufficient adhesion between the coating layers is required to improve the durability (long lifespan) of the firing support plate. The purpose of this specification is to provide a firing support plate for firing with improved durability, specifically for firing support plates having multiple layers of coating.

[0005] Methods for solving problems

[0006] One embodiment of the firing plate disclosed in this specification may include: a mullite layer, a first layer disposed on the mullite layer and comprising oxides containing Zr, Si and Y elements, and a yttrium oxide layer disposed on the first layer.

[0007] Another embodiment of the firing plate disclosed in this specification may include: a substrate formed of a material selected from SiC, Si-SiC and alumina; a first layer disposed on the substrate and comprising an oxide containing Zr and Y elements, as well as Si or Al elements; and a yttrium oxide layer disposed on the first layer. Attached Figure Description

[0008] Figure 1 This represents an EPMA (Si mapping) image of the surface of the firing plate used for firing.

[0009] Figure 2 An EPMA image (AI mapping) showing the surface of the firing plate used for firing.

[0010] Figure 3 An EPMA image (Y-map) showing the surface of the firing plate used for firing.

[0011] Figure 4 An EPMA image (Zr mapping) showing the surface of the firing plate used for firing.

[0012] Figure 5 An EPMA image (O-map) showing the surface of the firing plate used for firing.

[0013] Figure 6 An EPMA (Fe mapping) image of the surface of the firing plate used for firing.

[0014] Figure 7 This is a summary of the embodiments.

[0015] Figure 8 This is a summary of the embodiments.

[0016] Figure 9 This is a summary of the embodiments.

[0017] Figure 10 This is a summary of the embodiments.

[0018] Figure 11 This is a summary of the embodiments.

[0019] Figure 12 This is a summary of the embodiments.

[0020] Figure 13 This is a summary of the embodiments.

[0021] Figure 14 This is a summary of the embodiments. Detailed Implementation

[0022] The firing support plate disclosed in this specification has at least a first layer and a yttrium oxide layer on a substrate. Examples of substrate materials include mullite (mullite layer), alumina, SiC, and Si-SiC. When the substrate is mullite, the firing support plate can be understood as having a mullite layer (substrate), a first layer disposed on the mullite layer, and a yttrium oxide layer disposed on the first layer. In this case, a coating having a first layer and a yttrium oxide layer is formed on the mullite substrate. It should be noted that "Si-SiC" refers to a material primarily composed of SiC particles with metallic Si contained between the SiC particles.

[0023] When the substrate is not mullite (such as alumina, SiC, or Si-SiC), a mullite layer can be formed on the substrate, and a first layer and a yttrium oxide layer can be formed on the mullite layer. In this case, a coating having a mullite layer, a first layer, and a yttrium oxide layer is formed on the substrate. Alternatively, a mullite layer can be omitted from the substrate, and a coating having a first layer and a yttrium oxide layer can be formed on the substrate.

[0024] As a first approach, when the firing support plate for firing has a mullite layer (mullite substrate, or a mullite layer formed on a substrate), the first layer may be an oxide containing Zr, Si, and Y elements. Specifically, the first layer may contain 0.3% by mass or more and 2.0% by mass of Zr-containing oxide, 5% by mass or more and 30% by mass of Si-containing oxide, and 30% by mass or more and 50% by mass of Y-containing oxide. It should be noted that the Zr-containing oxide may be 0.5% by mass or more, 1% by mass or more, or 1.5% by mass or more. Furthermore, the Zr-containing oxide may be 1.5% by mass or less, 1% by mass or less, or 0.5% by mass or less. The Si-containing oxide may be 7% by mass or more, 10% by mass or more, 12% by mass or more, or 20% by mass or more. Furthermore, the oxides containing Si can be 25% by mass or less, 20% by mass or less, 15% by mass or less, 13% by mass or less, 10% by mass or less, or 6% by mass or less. The oxides containing Y can be 35% by mass or more, 40% by mass or more, or 45% by mass or more. Additionally, the oxides containing Y can be 45% by mass or less, 40% by mass or less, or 35% by mass or less.

[0025] As described above, in the firing support plate of the first embodiment, the first layer comprises both the element (Si) constituting the mullite layer and the element (Y) constituting the yttrium oxide layer. Therefore, by using an oxide containing Zr, Si, and Y elements as the first layer, the first layer is firmly bonded to the mullite layer, and consequently, also firmly bonded to the yttrium oxide layer. As a result, delamination is less likely to occur between the mullite layer and the first layer, and between the first layer and the yttrium oxide layer, thus improving the durability of the firing support plate. Furthermore, by improving the adhesion between the mullite layer and the first layer, and between the first layer and the yttrium oxide layer, it is also possible to suppress the penetration of components contained in the fired material into the coating.

[0026] Furthermore, when the firing plate for firing has a mullite layer, a second layer comprising oxides containing Al, Si, and Y elements can be provided between the first layer and the yttrium oxide layer. Specifically, the second layer may contain 3% to 20% by mass of Al-containing oxides, 5% to 30% by mass of Si-containing oxides, and 30% to 50% by mass of Y-containing oxides. It should be noted that the Al-containing oxides may be 5% or more by mass, 10% or more by mass, or 15% or more by mass. Additionally, the Al-containing oxides may be 16% or less by mass, 11% or less by mass, or 6% or less by mass. The Si-containing oxides may be 7% or more by mass, 10% or more by mass, 12% or more by mass, or 20% or more by mass. Additionally, the Si-containing oxides may be 25% or less by mass, 20% or less by mass, 15% or less by mass, 13% or less by mass, 10% or less by mass, or 6% or less by mass. Oxides containing Y can be 35% or more by mass, 40% or more by mass, or 45% or more by mass. Alternatively, oxides containing Y can be less than 45% by mass, less than 40% by mass, or less than 35% by mass.

[0027] When a first layer, a second layer, and a yttrium oxide layer are provided on a mullite layer (a mullite substrate, or a mullite layer as part of a coating), the total thickness of the yttrium oxide layer, the first layer, and the second layer can be 3 to 20 μm. In this case, when the total thickness of the first layer, the second layer, and the yttrium oxide layer is set to 100%, the thickness of the first layer can be 10% to 35% of the total thickness, the thickness of the second layer can be 15% to 35% of the total thickness, and the thickness of the yttrium oxide layer can be 30% to 70% of the total thickness. It should be noted that when the mullite layer is provided on the substrate as a coating, the thickness of the mullite layer can be 5 to 80 μm.

[0028] When a first layer, a second layer, and a yttrium oxide layer are provided on a mullite layer, the first layer contains both the elements constituting the mullite layer (Si) and the elements constituting the second layer (Si, Y). Furthermore, the second layer contains both the elements constituting the first layer (Si, Y) and the element constituting the yttrium oxide layer (Y). As a result, the adhesion between the mullite layer and the first layer, between the first layer and the second layer, and between the second layer and the yttrium oxide layer is improved, the durability of the firing support plate for firing is improved, and the penetration of components contained in the fired material into the coating is suppressed.

[0029] As a second approach, when the substrate is not mullite (alumina, SiC, Si-SiC, etc.) and a firing support plate for firing is not provided with a mullite layer on the substrate, a first layer is provided on the substrate. In this case, the first layer may be an oxide containing Zr and Y elements, as well as Si or Al elements. More specifically, when the substrate is a Si-containing material such as SiC or Si-SiC, the first layer may be an oxide containing Zr, Y, and Si elements. In this case, the first layer also contains both the element constituting the substrate (Si) and the element constituting the yttrium oxide layer (Y). The adhesion between the substrate and the first layer, and between the first layer and the yttrium oxide layer, is improved, the durability of the firing support plate for firing is improved, and the penetration of components contained in the fired product into the coating can be suppressed.

[0030] Furthermore, when the substrate is a material containing Al, such as alumina, the first layer can be an oxide containing Zr, Y, and Al. In this case, the first layer also contains both the element constituting the substrate (Al) and the element constituting the yttrium oxide layer (Y). The adhesion between the substrate and the first layer, and between the first layer and the yttrium oxide layer, is improved, the durability of the firing plate for firing is improved, and the penetration of components contained in the fired product into the coating can be suppressed.

[0031] When the substrate is a Si-containing material such as SiC or Si-SiC, the first layer, similar to the case where a first layer is provided on a mullite layer, may contain 0.3% to 2.0% by mass of Zr oxide, 5% to 30% by mass of Si oxide, and 30% to 50% by mass of Y oxide. Furthermore, when the substrate is an Al-containing material such as alumina, the first layer may contain 0.3% to 2.0% by mass of Zr oxide, 3% to 20% by mass of Al oxide, and 30% to 50% by mass of Y oxide.

[0032] It should be noted that when the substrate is not mullite (such as alumina, SiC, or Si-SiC) and the firing support plate for firing does not have a mullite layer on the substrate, a second layer can be provided between the first layer and the yttrium oxide layer on the substrate. The second layer can be an oxide containing Y and either Si or Al. As described above, when the substrate is a Si-containing material such as SiC or Si-SiC, the first layer can be an oxide containing Zr, Y, and Si. Therefore, when the substrate is a Si-containing material such as SiC or Si-SiC (the first layer is an oxide containing Zr, Y, and Si), the second layer can be an oxide containing both Y and Si. In this case, the second layer also contains both the elements constituting the first layer (Si and Y) and the element constituting the yttrium oxide layer (Y). Furthermore, as described above, when the substrate is an Al-containing material such as alumina, the first layer can be an oxide containing Zr, Y, and Al. Therefore, when the substrate is an alumina-containing material such as aluminum (the first layer is an oxide containing Zr, Y, and Al), the second layer can be an oxide containing both Y and Al. In this case, the second layer also contains both the elements constituting the first layer (Al and Y) and the element constituting the yttrium oxide layer (Y). In any case, the adhesion between the substrate and the first layer, between the first and second layers, and between the first layer and the yttrium oxide layer is improved, the durability of the firing support plate for firing is improved, and the penetration of components contained in the fired product into the coating is suppressed.

[0033] It should be noted that, in the case of the firing plate for firing in the second method, the second layer may have 3% to 20% by mass of oxides containing Al (or Si) and 30% to 50% by mass of oxides containing Y. Furthermore, in the case of the firing plate for firing in the second method, the total thickness of the yttrium oxide layer, the first layer, and the second layer may be 3 to 20 μm. When the total thickness of the first layer, the second layer, and the yttrium oxide layer is set to 100%, the thickness of the first layer may be 2% to 20% of the total thickness, the thickness of the second layer may be 2% to 20% of the total thickness, and the thickness of the yttrium oxide layer may be 60% to 69% of the total thickness.

[0034] Reference Figures 1-6 The identification and concentration calculation methods for the mullite layer, the first layer, the second layer, and the yttrium oxide layer are explained. Figure 1 EPMA image showing the Si composition of the surface layer of the firing plate used for firing. Figure 2 EPMA image representing Al component, Figure 3 EPMA image representing the Y component, Figure 4 EPMA image representing Zr composition. Figure 5 EPMA image representing the O component. Figure 6 EPMA image showing the Fe composition.

[0035] like Figures 1-6 As shown, based on the EPMA measurement results, the concentration of each component in the surface layer of the firing plate can be determined by the intensity of the color. In fact, through EPMA measurement, the concentration of each component in each area can be confirmed by referring to the color bars shown on the right side of the EPMA image. The distinction between the mullite layer, the first layer, the second layer, and the yttrium oxide layer is determined by the concentration of each component in each area. The mullite layer is the area where Si, Al, and O components are detected; specifically, a layer where Si content is 5% or higher, Al content is 10% or higher, and O content is 10% or higher is defined as the mullite layer. The first layer is the area where Zr, Si, and Y are detected, and it is the area where the Zr component concentration is higher than other areas. The second layer is the area where Y, Al, and Si are detected, and it is the area where the Al component concentration is higher than other areas at the location where it overlaps with the Y component. The yttrium oxide layer is the area closer to the surface and with a higher Y component concentration than the first layer, after the first layer has been determined. After identifying each layer (mullite layer, first layer, second layer, and yttrium oxide layer), the component concentrations of each layer were calculated using the color bars. It should be noted that, when the substrate is alumina, the first layer contains Zr, Al, and Y, and has a higher Zr concentration compared to other layers. The second layer contains Y and Al.

[0036] Example

[0037] Firing plates with different substrate and coating morphologies were manufactured to evaluate the coating adhesion and reactivity. Coating adhesion was evaluated using a peel test. In the peel test, commercially available adhesive tape was applied to the coating surface, and then forcefully peeled off. The state of the coating surface (the coating adhered to the tape) was visually confirmed. No visually confirmed peeling was designated as "A", peeling of less than 10% of the area was designated as "B", and peeling of more than 10% of the area was designated as "C". Coating reactivity was evaluated using a workpiece loading reaction test. In the workpiece loading reaction test, barium titanate was coated onto the coating surface and fired at 1200°C in atmospheric conditions for 2 hours. The reaction between the coating and the barium titanate was visually confirmed. Specifically, the surface of the fired coating was examined, and a melting or peeling state was considered a reaction. The case where no reaction was visually detected was designated as "A"; the case where a reaction was detected in an area less than 10% of the test area was designated as "B"; and the case where a reaction was detected in an area greater than 10% of the test area was designated as "C". The results are shown below. Figures 7-14 Additionally, in Figures 7-14The diagram also shows the mass ratio (concentration (%)) of the elements contained in each layer of the coating (mullite layer, first layer, second layer, and yttrium oxide layer) when converted to oxides, and the film thickness ratio of each layer. It should be noted that regarding... Figures 7-10 (Samples 1-18) When the total thickness of the first layer, the second layer and the yttrium oxide layer is set to 100%, it also represents the thickness ratio (%) of each layer.

[0038] Figures 7-9 This indicates the result of forming a coating on a substrate consisting of a mullite layer, a first layer, a second layer, and a yttrium oxide layer. Figure 7 The results show the use of Si-SiC substrates (samples 1-9). Figure 8 The results show the use of SiC substrate (samples 10–18). Figure 9 The results show the use of alumina substrate (samples 19–27). Figure 10 This indicates the results of coatings formed on a substrate, consisting of a mullite layer, a first layer, and a yttrium oxide layer (samples 28–36).

[0039] Figure 11 This indicates the result of a coating on a substrate in which a mullite layer is formed, and a yttrium oxide layer or a zirconium oxide layer is formed on top of the mullite layer without forming a first layer. Samples 37 and 38 represent the results using a Si-SiC substrate, samples 39 and 40 represent the results using a SiC substrate, and samples 41 and 42 represent the results using an alumina substrate.

[0040] Figures 12-14 This indicates the result of forming a coating with a first layer, a second layer, a yttrium oxide layer, or a zirconium oxide layer on the substrate without forming a mullite layer. Figure 12 The results show the use of Si-SiC substrates (samples 43–47). Figure 13 The results show the use of SiC substrate (samples 48–54). Figure 14 The results show the use of alumina substrate (samples 55-59). It should be noted that in samples 44, 45, 51, 52, 56, and 57, an alumina layer was formed in place of the mullite layer.

[0041] In samples 1-42, firstly, mullite particles were mixed with a solvent to prepare a mullite paste. Then, the mullite paste was printed onto the entire surface of the substrate with a thickness of 10 μm. After drying, it was fired at 1270℃-1350℃, thereby forming a mullite layer on the substrate. It should be noted that samples 1-10 used mullite particles with a particle size (D50) of 0.4 μm, samples 11-20 used mullite particles with a particle size (D50) of 0.7 μm, samples 21-30 used mullite particles with a particle size (D50) of 1.3 μm, samples 31-38 used mullite particles with a particle size (D50) of 0.5 μm, and samples 39-42 used mullite particles with a particle size (D50) of 0.6 μm. In addition, samples 1-10 were fired at 1270℃ for 2 hours, samples 11-20 at 1300℃ for 2 hours, samples 21-30 at 1350℃ for 2 hours, samples 31-38 at 1330℃ for 2 hours, and samples 39-42 at 1310℃ for 2 hours.

[0042] Regarding the method for forming the alumina layer in samples 44, 45, 51, 52, 56, and 57, alumina particles were mixed with a solvent to prepare an alumina paste. This alumina paste was then printed onto the entire surface of the substrate with a thickness of 8 μm. After drying, the paste was fired at 1350°C for 2 hours, thereby forming the alumina layer on the substrate. It should be noted that alumina particles with a particle size (D50) of 0.5 μm were used.

[0043] Next, yttrium oxide particles are mixed with an organic solvent to prepare a yttrium oxide paste. This paste is then printed onto the surface of the mullite layer to a thickness of 10 μm, dried, and fired at 1270℃–1350℃. It should be noted that during the yttrium oxide particle pulverization process, the required amounts of Al, Zr, and Si are uniformly added while pulverization is being carried out. Samples 1–10 used yttrium oxide particles with a particle size (D50) of 0.5 μm; samples 11–20 used yttrium oxide particles with a particle size (D50) of 0.9 μm; samples 21–30 used yttrium oxide particles with a particle size (D50) of 1.2 μm; samples 31–36 and 38 used yttrium oxide particles with a particle size (D50) of 0.6 μm; samples 40 and 42 used yttrium oxide particles with a particle size (D50) of 0.8 μm; samples 43, 44, 46, and 48–50 used yttrium oxide particles with a particle size (D50) of 0.5 μm; and samples 51, 53, 55, 56, and 58 used yttrium oxide particles with a particle size (D50) of 0.6 μm. In addition, samples 1-10 were fired at 1270℃ for 2 hours, samples 11-20 at 1330℃ for 2 hours, samples 21-30 at 1350℃ for 2 hours, samples 31-38 at 1310℃ for 2 hours, samples 39-42 at 1290℃ for 2 hours, samples 43-50 at 1320℃ for 2 hours, and samples 51-59 at 1350℃ for 2 hours. Samples 1-51 with different compositions for each layer were prepared by changing the particle size of the raw material particles (mullite particles and yttrium oxide particles) and the firing time. It should be noted that for samples 2, 11, and 20, zirconium oxide particles were added to the yttrium oxide particles during the preparation of the yttrium oxide paste. Furthermore, for samples 37, 39, 41, 45, 47, 52, 54, 57, and 59, zirconium oxide paste was used instead of yttrium oxide paste. It should be noted that the thickness of the yttrium oxide layer (or zirconium oxide layer) (after firing) is 10 μm. Furthermore, in the presence of the yttrium oxide layer, the first layer, and the second layer, the total thickness of the yttrium oxide layer, the first layer, and the second layer is 10 μm.

[0044] As shown in samples 1-27, when the coating has a first layer, a second layer, and a yttrium oxide layer, both film adhesion and film reactivity are rated "A". On the other hand, samples (samples 37-42) with a mullite layer formed on the substrate but without a first layer cannot achieve "A" ratings for both film adhesion and film reactivity. These results confirm that by providing a first layer on the mullite layer and then providing a yttrium oxide layer on the first layer, both film adhesion and film reactivity are improved.

[0045] Furthermore, the film adhesion of samples (samples 43, 48, 49, 50, and 55) that had a first layer but no mullite layer on the substrate was rated "B," and their film reactivity was rated "A." It should be noted that the film adhesion and film reactivity of samples (samples 44, 45, 51, 52, 56, and 57) that had an alumina layer on the substrate instead of a mullite layer were both rated "B." The film adhesion and film reactivity of samples (samples 46, 53, and 58) that had a yttrium oxide layer directly formed on the substrate were both rated "B." Among the samples (samples 47, 54, and 59) with a zirconium oxide layer directly formed on the substrate, the sample using an alumina substrate (sample 59) received a "B" rating for both film adhesion and film reactivity, while the others received a "C" rating for both.

[0046] The specific examples of the present invention have been described in detail above, but these are merely illustrative and do not limit the scope of protection claimed in the claims. The technology described in the claims includes technologies modified or altered from the specific examples described above. Furthermore, the technical elements described in this specification or drawings are useful individually or in various combinations, and are not limited to the combinations described in the claims at the time of application. Additionally, the technology illustrated in this specification or drawings can achieve multiple objectives simultaneously, and achieving one of these objectives is itself technically useful.

Claims

1. A firing support plate for firing, comprising: A substrate layer formed from materials selected from SiC, Si-SiC, and alumina. Mullite layers The first layer, set on top of the mullite layer, is an oxide containing Zr, Si, and Y elements, and The second layer, located on top of the first layer, is an oxide containing Al, Si, and Y elements. A yttrium oxide layer disposed on the second layer, The first layer contains 0.3% to 2.0% by mass of oxides containing Zr, 5% to 30% by mass of oxides containing Si, and 30% to 50% by mass of oxides containing Y. The second layer contains 3% to 20% by mass of oxides containing Al, 5% to 30% by mass of oxides containing Si, and 30% to 50% by mass of oxides containing Y.

2. The firing support plate according to claim 1, wherein, The first layer contains 0.5% to 1.5% by mass of oxides containing Zr, 7% to 15% by mass of oxides containing Si, and 45% to 50% by mass of oxides containing Y.

3. The firing support plate according to claim 1, wherein the second layer comprises 5% by mass and 16% by mass of an oxide containing Al, 5% by mass and 15% by mass of an oxide containing Si, and 45% by mass and 50% by mass of an oxide containing Y.

4. The firing support plate according to claim 1 or 2, wherein, When the total thickness of the first layer, the second layer, and the yttrium oxide layer is set to 100%, the thickness of the first layer is 10% or more and 35% or less, the thickness of the second layer is 15% or more and 35% or less, and the thickness of the yttrium oxide layer is 30% or more and 70% or less.

5. The firing support plate according to claim 4, wherein, The combined thickness of the yttrium oxide layer, the first layer, and the second layer is 3~20 μm.

6. The firing support plate according to claim 1, wherein, A mullite layer is formed as a coating on a SiC substrate.

Citation Information

Patent Citations

  • Calcination tool for electronic parts

    JP2002154884A

  • Information processing device and information processing method

    JP2022051967A

  • Calcination jig

    CN113383204A

  • Laminate, corrosion resistant member and halogen gas plasma resistant member

    JP2002001865A

  • Firing setter

    WO2022049980A1