一种复合型铸造涂料配方及其制备方法

A composite casting coating prepared by using a specific ratio of zircon powder, flake graphite powder, mica powder and other materials solves the defects of sand adhesion and cold shut in the steel casting process and improves the surface quality of castings.

CN118513500BActive Publication Date: 2026-11-24WUXI INSTITUTE OF TECHNOLOGY
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410765495.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2026-11-24
Estimated Expiration
2044-06-14

AI Technical Summary

Technical Problem

During the steel casting process, there are defects such as sand adhesion during pouring and slight cold shut defects at the thin-walled positions at the far end of complex structural products, which affect the surface quality of the castings.

Method used

A composite casting coating is prepared by using zircon powder, flake graphite powder, and mica powder in specific proportions as the main aggregates, and adding suspending agents, binders, surfactants, preservatives, defoamers, rheology modifiers, and water through specific stirring steps, thereby improving the coating's high temperature resistance and thermal insulation properties.

Benefits of technology

It effectively solves the sand adhesion defect in the steel casting process and the cold shut defect at the far end of the thin wall of complex structure products, and improves the surface quality of castings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure REF-OBJ-1791797358151-000001
    Figure REF-OBJ-1791797358151-000001
  • Figure REF-OBJ-1791797358151-000002
    Figure REF-OBJ-1791797358151-000002
Patent Text Reader

Abstract

The application relates to the technical field of metal material liquid forming, and discloses a composite casting coating formula and a preparation method thereof. In the application, zirconium powder, phosphorus flake graphite powder and mica powder are selected as main aggregates in specific contents, and ferroferric oxide powder is selected in a specific content, and auxiliary materials such as suspending agents, binders, surfactants, preservatives, defoaming agents and rheological aids are introduced, the prepared composite casting coating has good high-temperature resistance and heat insulation, the obtained composite casting coating can solve the sand sticking defects on the surface of cast steel products and the slight cold shut defects of thin walls of complex structure products, so that the surface quality of the castings is improved, and high-quality castings are produced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of liquid metal forming technology, specifically to a composite casting coating formulation and its preparation method. Background Technology

[0002] Sand casting is a widely used casting method in various industries such as automobiles and machine tools. While unaffected by the material of the product, sand casting can produce both simple and complex castings.

[0003] In casting products, the pouring temperature of cast steel is generally higher than that of cast iron. Therefore, during the steel casting process, the sand core is often encased in molten iron, making it prone to casting defects such as sand adhesion. Furthermore, the surface of the casting blank is affected by the sand mold and sand core, resulting in a relatively rough finished product. Additionally, for products with complex structures, cold shut defects are prone to occur when molten steel fills to the thin-walled areas at the far ends of the mold. Summary of the Invention

[0004] The purpose of this invention is to overcome the defects of sand adhesion during the casting process and slight cold shut defects at the far end of the casting that exist in existing steel casting technology.

[0005] The technical solution adopted is as follows: A first aspect of the present invention provides a composite casting coating formulation, the coating formulation comprising the following components: Zircon powder, flake graphite powder, mica powder, ferric oxide powder, suspending agent, binder, surfactant, preservative, defoamer, rheology modifier, water; Based on the total mass of the coating formulation, the content of zircon powder is 19-22 wt%, the content of flake graphite powder is 3-6 wt%, the content of mica powder is 39-42 wt%, the content of ferric oxide powder is 2-5 wt%, the content of suspending agent is 0.9-2.3 wt%, the content of binder is 4-7 wt%, the content of surfactant is 0.35-0.75 wt%, the content of preservative is 0.1-0.5 wt%, the content of defoamer is 0.2-0.45 wt%, the content of rheology modifier is 0.13-0.35 wt%, and the content of water is 14.65-31.32 wt%.

[0006] Preferably, the zircon powder is 200 mesh, 300 mesh, or 325 mesh.

[0007] Preferably, the phosphorus flake graphite powder is 100 mesh or 150 mesh.

[0008] More preferably, the mica powder is 60 mesh, 70 mesh, or 80 mesh.

[0009] A second aspect of the present invention provides a method for preparing the composite casting coating formulation described in the first aspect of the present invention, the method comprising the following steps: (1) Add water to the mixing tank, and add binder, preservative, surfactant and rheology modifier, and carry out the first stirring to obtain mixture I; the conditions for the first stirring should at least meet the following: time is 10~15min; (2) The suspending agent is added to the mixture I and stirred for a second time to obtain mixture II; the conditions for the second stirring are at least: the time is 10~15 min; (3) Add zircon powder and ferric oxide powder to the mixture II and stir for the third time to obtain mixture III; the conditions for the third stirring are at least: the time is 10~15min; (4) Add the phosphorus flake graphite powder and mica powder to the mixture III and stir for the fourth time to obtain the mixture IV; the conditions for the fourth stirring shall at least meet the following: first stir at a speed of 300 r / min for 10 to 150 min, and then stir at a speed of 1500 r / min for 30 to 40 min. (5) Add the defoamer to the mixture IV and stir for the fifth time to obtain mixture V; the conditions for the fifth stirring are at least: the time is 10~15min; (6) Add water to the mixture V, perform a sixth stirring, and then fill it into a container; the conditions for the sixth stirring are at least: the time is 10~15min.

[0010] Preferably, the conditions for the first stirring, the second stirring, the third stirring, the fifth stirring, and the sixth stirring also satisfy the following: the stirring speed is 700 r / min.

[0011] The beneficial effects of this invention are: In this invention, zircon powder, flake graphite powder, and mica powder with specific contents are selected as the main aggregates, along with ferric oxide powder with a specific content. Suspension agents, binders, surfactants, preservatives, defoamers, rheology modifiers, and other auxiliary materials are introduced. Testing shows that the resulting composite casting coating exhibits good high-temperature resistance and thermal insulation properties. Furthermore, the composite casting coating can resolve surface sand adhesion defects in cast steel products and address minor cold shut defects at the far ends of complex structural products, thereby improving the surface quality of castings and producing high-quality castings. Detailed Implementation

[0012] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0013] It should be noted that, in all aspects of the present invention, the same components in each aspect are described only once in one aspect and not repeatedly, and those skilled in the art should not understand this as a limitation of the present invention.

[0014] As previously described, a first aspect of the present invention provides a composite casting coating formulation, the coating formulation comprising the following components: Zircon powder, flake graphite powder, mica powder, ferric oxide powder, suspending agent, binder, surfactant, preservative, defoamer, rheology modifier, water; Based on the total mass of the coating formulation, the content of zircon powder is 19-22 wt%, the content of flake graphite powder is 3-6 wt%, the content of mica powder is 39-42 wt%, the content of ferric oxide powder is 2-5 wt%, the content of suspending agent is 0.9-2.3 wt%, the content of binder is 4-7 wt%, the content of surfactant is 0.35-0.75 wt%, the content of preservative is 0.1-0.5 wt%, the content of defoamer is 0.2-0.45 wt%, the content of rheology modifier is 0.13-0.35 wt%, and the content of water is 14.65-31.32 wt%.

[0015] It should be noted that, in the research process of this invention, in order to solve the defects of sand adhering to the inner cavity of castings and slight cold shut defects in thin-walled products of complex structures that occur during the casting process in existing steel casting technology, the technical solution of this invention uses zircon powder, which has high temperature resistance, mica powder, which has heat insulation properties, and flake graphite powder, which has good lubricity. Using zircon powder, flake graphite powder, and mica powder as the main aggregates can solve the sand adhering defects that are easily caused by excessive temperature in steel castings and the slight cold shut defects in thin-walled products of complex structures, thereby preparing a composite casting coating with excellent performance.

[0016] In this invention, the zircon powder content is a crucial factor. Excessive zircon powder content, due to its relatively rapid cooling properties, can cause a temperature drop in the molten steel within the mold cavity. Conversely, insufficient zircon powder content lacks adequate high-temperature resistance, leading to sand adhesion within the casting cavity. The inventors of this invention have discovered that, based on the total mass of the coating, a zircon powder content of 19-22 wt%, combined with other technical features of this invention, can reduce the temperature drop of the molten steel while maintaining good high-temperature resistance and preventing sand adhesion.

[0017] In this invention, the content of mica powder is a crucial factor. Excessive mica powder content can lead to sand adhesion within the casting cavity due to mica's relatively poor high-temperature resistance; conversely, insufficient mica powder content results in inadequate thermal insulation, failing to provide adequate insulation. The inventors of this invention have discovered that, based on the total mass of the coating, a mica powder content of 39-42 wt%, combined with the other technical features of this invention, achieves superior thermal insulation (reducing the temperature drop of the molten steel).

[0018] Preferably, the zircon powder is 200 mesh, 300 mesh, or 325 mesh.

[0019] Preferably, the phosphorus flake graphite powder is 100 mesh or 150 mesh.

[0020] More preferably, the mica powder is 60 mesh, 70 mesh, or 80 mesh.

[0021] In this invention, the zircon powder is 200 mesh, 300 mesh, or 325 mesh; the phosphorus flake graphite powder is 100 mesh or 150 mesh; and the mica powder particles are 60 mesh, 70 mesh, or 80 mesh. The inventors of this invention have discovered that, under these preferred conditions, in conjunction with the other technical features of this invention, when applied to phenolic resin sand cores / molds, the gaps between the sand particles in the phenolic resin sand cores / molds can be completely filled, and the phenolic resin can penetrate into the phenolic resin sand cores / molds by approximately 3 mm.

[0022] In this invention, water is chosen as the carrier liquid because water-based coatings are safer and more environmentally friendly than alcohol-based coatings during production and use.

[0023] In this invention, there are no particular requirements regarding the types of suspending agents, binders, surfactants, preservatives, defoamers, and rheology modifiers; all are common materials in the art. For example, the suspending agent is needle-shaped bentonite, the binder is an emulsion or modified starch, the surfactant is a dispersant, and the preservative is an aldehyde preservative. Further details are omitted here, and those skilled in the art should not construe this as a limitation of the invention.

[0024] As described above, a second aspect of the present invention provides a method for preparing the composite casting coating formulation described in the first aspect of the present invention, the method comprising the following steps: (1) Add water to the mixing tank, and add binder, preservative, surfactant and rheology modifier, and carry out the first stirring to obtain mixture I; the conditions for the first stirring should at least meet the following: time is 10~15min; (2) The suspending agent is added to the mixture I and stirred for a second time to obtain mixture II; the conditions for the second stirring are at least: the time is 10~15 min; (3) Add zircon powder and ferric oxide powder to the mixture II and stir for the third time to obtain mixture III; the conditions for the third stirring are at least: the time is 10~15min; (4) Add the phosphorus flake graphite powder and mica powder to the mixture III and stir for the fourth time to obtain the mixture IV; the conditions for the fourth stirring shall at least meet the following: first stir at a speed of 300 r / min for 10 to 150 min, and then stir at a speed of 1500 r / min for 30 to 40 min. (5) Add the defoamer to the mixture IV and stir for the fifth time to obtain mixture V; the conditions for the fifth stirring are at least: the time is 10~15min; (6) Add water to the mixture V, perform a sixth stirring, and then fill it into a container; the conditions for the sixth stirring are at least: the time is 10~15min.

[0025] Preferably, the conditions for the first stirring, the second stirring, the third stirring, the fifth stirring, and the sixth stirring also satisfy the following: the stirring speed is 700 r / min.

[0026] The present invention will be described in detail below through examples. In the following examples, unless otherwise specified, the raw materials are all commercially available products.

[0027] Example 1

[0028] A composite casting coating formulation, comprising the following components by weight: Zircon powder, flake graphite powder, mica powder, ferric oxide powder, suspending agent, binder, surfactant, preservative, defoamer, rheology modifier, water.

[0029] The preparation method of the composite casting coating formulation is as follows (according to the formulation and process parameters in Table 1): (1) Add water to the mixing tank, and add binder, preservative, surfactant and rheology modifier, and carry out the first stirring to obtain mixture I; (2) The suspending agent is added to the mixture I and stirred for a second time to obtain mixture II; (3) Add zircon powder and ferric oxide powder to the mixture II and stir for the third time to obtain mixture III; (4) Add the phosphorus flake graphite powder and mica powder to the mixture III and stir for the fourth time to obtain mixture IV; (5) Add the defoamer to the mixture IV and stir for the fifth time to obtain mixture V; (6) Add water to the mixture V, stir for the sixth time, and then fill it into a container.

[0030] Unless otherwise specified, Comparative Examples 1, 2 and 4 were carried out using the same process as Example 1, but the formulations and process parameters used were different, as detailed in Table 1.

[0031] Table 1

[0032] Test Example 1 The composite casting coating formulations obtained in the above embodiments and comparative examples were used for phenolic resin sand core impregnation coating. The minimum wall thickness of the sand core was 5 mm, and the wall thickness of the thin-walled part of the casting was 5 mm. A total of 31 casting tests were conducted, and the results are shown in Table 2.

[0033] Table 2

[0034] As can be seen from the results in Table 2, the composite casting coating prepared by the present invention has significantly better effects. Specifically, no sand adhesion defects occurred in the casting cavity during the casting process, and no cold shut defects occurred in the thin-walled part of the casting.

[0035] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A composite casting coating formulation, characterized in that, The coating formulation includes the following components: Zircon powder, flake graphite powder, mica powder, ferric oxide powder, suspending agent, binder, surfactant, preservative, defoamer, rheology modifier, water; Based on the total mass of the coating formulation, the content of zircon powder is 21 wt%, the content of flake graphite powder is 5 wt%, the content of mica powder is 41 wt%, the content of ferric oxide powder is 4 wt%, the content of suspending agent is 1.8 wt%, the content of binder is 5.5 wt%, the content of surfactant is 0.6 wt%, the content of preservative is 0.38 wt%, the content of defoamer is 0.35 wt%, the content of rheology modifier is 0.28 wt%, and the content of water is 20.09 wt%.

2. The composite casting coating formulation according to claim 1, wherein, The zircon powder is 200 mesh, 300 mesh, or 325 mesh.

3. The composite casting coating formulation according to claim 1 or 2, wherein, The phosphorus flake graphite powder is 100 mesh or 150 mesh.

4. The composite casting coating formulation according to claim 1 or 2, wherein, The mica powder is 60 mesh, 70 mesh, or 80 mesh.

5. A method for preparing a composite casting coating formulation as described in any one of claims 1-4, characterized in that, The method includes the following steps: (1) Add water to the mixing tank, and add binder, preservative, surfactant and rheology modifier, and carry out the first stirring to obtain mixture I; the conditions for the first stirring shall at least meet the following: time is 15 min; (2) The suspending agent is added to the mixture I and stirred for a second time to obtain mixture II; the conditions for the second stirring are at least: the time is 15 min; (3) Add zircon powder and ferric oxide powder to the mixture II and stir for the third time to obtain mixture III; the conditions for the third stirring are at least: the time is 15 min; (4) Add the phosphorus flake graphite powder and mica powder to the mixture III and stir for the fourth time to obtain the mixture IV; the conditions for the fourth stirring shall at least meet the following: first stir at a speed of 300 r / min for 150 min, and then stir at a speed of 1500 r / min for 30 min. (5) Add the defoamer to the mixture IV and stir for the fifth time to obtain mixture V; the conditions for the fifth stirring are at least: the time is 15 min; (6) Add water to the mixture V, perform a sixth stirring, and then fill it into a container; the conditions for the sixth stirring must be at least: the time is 15 minutes.

6. The method according to claim 5, wherein, The conditions for the first stirring, the second stirring, the third stirring, the fifth stirring, and the sixth stirring also satisfy the following: the stirring speed is 700 r / min.

Citation Information

Patent Citations

  • Preparation method of sand core dip-coating coating and prepared coating

    CN109746385A

  • Coating for sand core of gray iron cylinder body of automobile engine and preparation method of coating