High-aluminum uniformly doped large-particle cobalt carbonate, and preparation method and application thereof

By controlling the injection flow rate and temperature of the cobalt-aluminum mixed salt solution and the precipitant solution through a co-precipitation method, high-aluminum uniformly doped large-particle cobalt carbonate was prepared, solving the problems of uneven aluminum distribution and low production efficiency in the existing technology, and improving the electrical performance and production efficiency of lithium cobalt oxide materials.

CN118515319BActive Publication Date: 2026-11-20JINGMEN GEM NEW MATERIAL CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410839439.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2026-11-20
Estimated Expiration
2044-06-26

AI Technical Summary

Technical Problem

Existing technologies make it difficult to prepare large-particle cobalt carbonate with uniform high aluminum doping, which leads to the degradation of the electrical properties of lithium cobalt oxide materials under high voltage, and also results in low production efficiency and high cost.

Method used

The co-precipitation method is adopted. First, a first co-precipitation reaction is carried out to achieve the target particle size of 10-15μm. Then, the co-flow rate of the co-cobalt aluminum mixed salt solution and the precipitant solution and the reaction temperature are reduced to control the second co-precipitation reaction, so as to realize the phase transformation of blocky primary particles into lamellar primary particles, avoid the explosion of small particles, and ensure the uniform distribution of aluminum elements.

Benefits of technology

High-alumina uniformly doped large-particle cobalt carbonate with a particle size of 20-23 μm was prepared, which improved the electrical performance of lithium cobalt oxide cathode material under high voltage, reduced calcination process time, improved production efficiency, and reduced energy costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118515319B_ABST
    Figure CN118515319B_ABST
Patent Text Reader

Abstract

This invention provides a method for preparing high-alumina uniformly doped large-particle cobalt carbonate. The method is based on coprecipitation. First, a first coprecipitation reaction is carried out to achieve a first target particle size of 10-15 μm. Then, the co-current injection flow rates of the cobalt-aluminum mixed salt solution and the precipitant solution are reduced, and the reaction temperature is lowered, which reduces the reactivity of the second coprecipitation reaction. This achieves the phase transition from blocky primary particles to lamellar primary particles, which is beneficial to the adhesion and accumulation of lamellar primary particles and avoids small particle bursts. Thus, high-alumina uniformly doped large-particle cobalt carbonate with a particle size of 20-23 μm can be obtained. Since the concentrations of the cobalt-aluminum mixed salt solution and the precipitant solution remain unchanged, the aluminum concentration of the entire cobalt carbonate particle is uniform.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery technology, specifically to lithium cobalt oxide batteries, and more particularly to a high-aluminum uniformly doped large-particle cobalt carbonate, its preparation method, and its application. Background Technology

[0002] Lithium-ion batteries, with their core advantages of high energy density, high power density, and high safety performance, are widely used in consumer electronics, power tools, energy storage, aerospace, and other fields, making them the fastest-growing and most promising new energy storage technology. With advancements in technology and expanding energy demands, developing next-generation lithium-ion batteries with even higher energy density has become a top priority. Among these technologies, cathode materials are the key technological bottleneck determining battery energy density and account for more than one-third of the total cost of lithium-ion batteries. Therefore, researching and developing lower-cost, higher-capacity cathode materials is one of the important development goals of lithium-ion battery technology.

[0003] Among commercially available cathode materials, layered lithium cobalt oxide boasts the highest energy density and is the most competitive and promising cathode material for achieving next-generation lithium-ion batteries with higher energy density. However, as the earliest commercially available cathode material, lithium cobalt oxide's large-scale commercialization level is currently limited to below 4.6V, and there remains a gap between its actual discharge capacity and theoretical capacity. Further increasing the operating cutoff voltage can improve lithium-ion utilization, thereby increasing discharge capacity and energy density. Therefore, the development of modification technologies for high-voltage lithium cobalt oxide is a hot topic of common interest in both academia and industry.

[0004] From a bulk perspective, at high voltages, especially above 4.55V, the bulk phase undergoes an incompletely reversible H3-M2 phase transition, leading to drastic changes in cell parameters and lattice distortion, which can easily cause problems such as cracks and particle breakage. On the other hand, the surface stability of lithium cobalt oxide is also precarious under high voltage due to multiple factors, thus affecting the electrical performance of lithium cobalt oxide materials.

[0005] Domestically developed lithium cobalt oxide materials often experience performance degradation at 4.55V, so various methods are employed to increase the voltage plateau and thus improve capacity. Al doping is one such method. However, as the Al doping content increases, the internal distribution often becomes uneven, ultimately affecting the material's battery performance.

[0006] CN105399148A discloses a method for preparing large-particle-size, high-density spherical cobalt tetroxide. The method includes a cobalt carbonate synthesis stage and a spherical cobalt carbonate thermal decomposition stage. In the cobalt carbonate synthesis stage, the cobalt carbonate precursor obtained through multiple cycles of crystallization is relatively dense and has a uniform particle size distribution, yielding spherical cobalt carbonate with a crystal particle size of 18-23 μm. However, this method uses a clarification process for both seed crystal preparation and post-processing production, which cannot be continuous. This results in low efficiency, low cobalt metal recovery, unstable products, and a high likelihood of producing small particles or lumps.

[0007] CN108649219A discloses a method for preparing large-particle-size aluminum-doped cobalt tetroxide. The method includes: continuously and simultaneously adding an aluminum-cobalt solution and an ammonium bicarbonate solution to a reaction vessel for neutralization and precipitation, while simultaneously separating the supernatant free of material to obtain cobalt carbonate seed crystals with an aluminum particle size (D50) of 10–14.5 μm. Then, aluminum-cobalt solution and ammonium bicarbonate solution are added to the seed crystals for further neutralization and precipitation until large-particle-size aluminum-doped cobalt carbonate with a D50 of 18–21 μm is obtained. However, this method employs a semi-continuous process, resulting in a relatively low aluminum doping level, which cannot meet the requirements of high voltage, and does not offer a good solution for high-aluminum doping.

[0008] When preparing aluminum-doped large-particle cobalt carbonate using a continuous co-precipitation process, a problem of small particle bursts often occurs in the later stages of the reaction. The small particles generated by the bursts do not easily adhere to and accumulate on the cobalt carbonate particles generated in the earlier stages, and often exist in a free state. This makes it difficult to prepare large-particle cobalt carbonate with uniform particle size. Moreover, aluminum is more likely to be doped on the free small particles, resulting in uneven aluminum distribution and deviation of aluminum content from the target content.

[0009] Therefore, there is a need to develop a high-alumina uniformly doped large-particle cobalt carbonate, its preparation method, and its applications. Summary of the Invention

[0010] In view of the problems existing in the prior art, the present invention provides a method for preparing high-alumina uniformly doped large-particle cobalt carbonate. The preparation method is based on co-precipitation. First, a first co-precipitation reaction is performed to achieve a first target particle size of 10-15 μm. Then, the co-flow rate of the cobalt-aluminum mixed salt solution and the precipitant solution is reduced, and the reaction temperature is lowered, thereby reducing the reactivity of the second co-precipitation reaction. This achieves the phase transformation from blocky primary particles to lamellar primary particles, which is beneficial for the adhesion and accumulation of lamellar primary particles and avoids small particle bursts. This yields high-alumina uniformly doped large-particle cobalt carbonate with a particle size of 20-23 μm. Because the concentrations of the cobalt-aluminum mixed salt solution and the precipitant solution remain constant, the aluminum concentration of the entire cobalt carbonate particle is uniform. Using the high-alumina uniformly doped large-particle cobalt carbonate prepared by the present invention to prepare lithium cobalt oxide cathode materials can not only improve the electrical performance of the cathode material under high voltage, but also reduce the time of the subsequent calcination process, improve efficiency, and save energy costs for mass production.

[0011] To achieve this objective, the present invention adopts the following technical solution:

[0012] One objective of this invention is to provide a method for preparing high-alumina uniformly doped large-particle cobalt carbonate, the method comprising the following steps:

[0013] A cobalt-aluminum mixed salt solution and a precipitant solution are injected concurrently into the reaction substrate to carry out the first coprecipitation reaction. After the first target particle size of 10-15 μm is achieved, the concurrent injection flow rate of the cobalt-aluminum mixed salt solution and the precipitant solution is reduced, and the reaction temperature is lowered to carry out the second coprecipitation reaction, thereby obtaining high-aluminum uniformly doped large-particle cobalt carbonate with a particle size of 20-23 μm.

[0014] The preparation method described in this invention is based on a co-precipitation method. First, a first co-precipitation reaction is carried out to achieve a first target particle size of 10-15 μm. Then, the co-flow rate of the cobalt-aluminum mixed salt solution and the precipitant solution is reduced, and the reaction temperature is lowered, which reduces the reactivity of the second co-precipitation reaction. This achieves the phase transformation from blocky primary particles to lamellar primary particles, which is beneficial to the adhesion and accumulation of lamellar primary particles and avoids the bursting of small particles. As a result, high-aluminum uniformly doped large-particle cobalt carbonate with a particle size of 20-23 μm can be obtained. Since the concentrations of the cobalt-aluminum mixed salt solution and the precipitant solution remain unchanged, the aluminum concentration of the entire cobalt carbonate particle is uniform.

[0015] The preparation method described in this invention selects a first target particle size of 10-15 μm as the standard for primary particle phase inversion, which can ensure that the final cobalt carbonate has good sphericity and that the outermost lamellar primary particles can achieve a certain density, thus achieving good adhesion and stacking. If the first target particle size is <10 μm, the primary particle phase inversion occurs too early, which will result in insufficient sphericity of the secondary particles obtained by the stacking of the primary particles, with an uneven surface and uneven distribution of aluminum. If the first target particle size is >15 μm, the primary particle phase inversion occurs too late, which will cause small particles to start to explode, and the outermost lamellar primary particles will be very loose, making them prone to cracking and breakage.

[0016] It should be noted that the first target particle size in the preparation method of the present invention is 10-15 μm, such as 10 μm, 11 μm, 12 μm, 13 μm, 14 μm or 15 μm, but is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0017] It should be noted that the particle size of the high-alumina uniformly doped large-particle cobalt carbonate in the preparation method of the present invention is 20-23 μm, such as 20 μm, 20.5 μm, 21 μm, 21.5 μm, 22 μm, 22.5 μm or 23 μm, but it is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0018] As a preferred embodiment of the present invention, the pH value of the first coprecipitation reaction is lower than the pH value of the second coprecipitation reaction.

[0019] In the preparation method described in this invention, it is preferable that the pH value of the first coprecipitation reaction is lower than that of the second coprecipitation reaction, that is, the pH value of the second stage of the coprecipitation reaction increases, which is more conducive to the formation of basic cobalt carbonate.

[0020] As a preferred technical solution of the present invention, the cobalt concentration in the cobalt-aluminum mixed salt solution is 1.8-2 mol / L, such as 1.8 mol / L, 1.9 mol / L or 2 mol / L, but is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0021] Preferably, the cobalt salt in the cobalt-aluminum mixed salt solution includes at least one of cobalt sulfate, cobalt nitrate, or cobalt chloride.

[0022] Preferably, the aluminum concentration in the cobalt-aluminum mixed salt solution is 57-115 mmol / L, such as 57 mmol / L, 60 mmol / L, 70 mmol / L, 80 mmol / L, 90 mmol / L, 100 mmol / L, 110 mmol / L, or 115 mmol / L, but is not limited to the listed values; other unlisted values ​​within the above range are also applicable.

[0023] Preferably, the aluminum salt in the cobalt-aluminum mixed salt solution includes at least one of aluminum sulfate, aluminum nitrate, or aluminum chloride.

[0024] Preferably, the precipitant solution includes at least one of ammonium carbonate, ammonium bicarbonate, sodium carbonate, or sodium bicarbonate.

[0025] Preferably, the concentration of the precipitant solution is 2-3 mol / L, such as 2 mol / L, 2.1 mol / L, 2.3 mol / L, 2.5 mol / L, 2.7 mol / L, 2.8 mol / L or 3 mol / L, but it is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0026] As a preferred embodiment of the present invention, in the first coprecipitation reaction, the injection flow rate of the cobalt-aluminum mixed salt solution is 25-40 mL / h, such as 25 mL / h, 30 mL / h, 35 mL / h or 40 mL / h, and the injection flow rate of the precipitant solution is 45-60 mL / h, such as 45 mL / h, 50 mL / h, 55 mL / h or 60 mL / h, but is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0027] Preferably, the reaction temperature of the first coprecipitation reaction is 43-47°C, such as 43°C, 44°C, 45°C, 46°C or 47°C, but it is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0028] As a preferred technical solution of the present invention, the stirring rate of the first coprecipitation reaction is 300-350 rpm, such as 300 rpm, 310 rpm, 320 rpm, 330 rpm, 340 rpm or 350 rpm, but is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0029] Preferably, the pH value of the first coprecipitation reaction is 6.7-7.8, such as 6.7, 6.8, 7.0, 7.2, 7.4, 7.6 or 7.8, but is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0030] As a preferred embodiment of the present invention, in the second coprecipitation reaction, the injection flow rate of the cobalt-aluminum mixed salt solution is 8-12 mL / h, such as 8 mL / h, 9 mL / h, 10 mL / h, 11 mL / h or 12 mL / h, etc., and the injection flow rate of the precipitant solution is 12-20 mL / h, such as 12 mL / h, 14 mL / h, 16 mL / h, 18 mL / h or 20 mL / h, etc., but is not limited to the listed values, and other unlisted values ​​within the above range are also applicable.

[0031] Preferably, the reaction temperature of the second coprecipitation reaction is 38-42°C, such as 38°C, 39°C, 40°C, 41°C or 42°C, but it is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0032] As a preferred technical solution of the present invention, the stirring rate of the second coprecipitation reaction is 200-230 rpm, such as 200 rpm, 210 rpm, 220 rpm or 230 rpm, but is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0033] Preferably, the pH value of the second coprecipitation reaction is 6.8-7.5, such as 6.8, 6.9, 7.0, 7.1, 7.2, 7.3, 7.4 or 7.5, but is not limited to the listed values. Other unlisted values ​​within the above range are also applicable.

[0034] It should be noted that, in the preparation method of the present invention, after the second coprecipitation reaction is completed, solid-liquid separation, washing and drying are performed sequentially; the washing process includes: the reaction liquid obtained from the second coprecipitation reaction is fed into a centrifuge for washing, and hot water and ammonium bicarbonate are used as washing media; the drying process includes: the washed material is dried in an oven at 100-150°C, and finally high-alumina uniformly doped large-particle cobalt carbonate is obtained.

[0035] As a preferred technical solution of the present invention, the preparation method includes the following steps:

[0036] Prepare a cobalt-aluminum mixed salt solution and a precipitant solution; the cobalt concentration in the cobalt-aluminum mixed salt solution is 1.8-2 mol / L, and the cobalt salt in the cobalt-aluminum mixed salt solution includes at least one of cobalt sulfate, cobalt nitrate, or cobalt chloride; the aluminum concentration in the cobalt-aluminum mixed salt solution is 57-115 mmol / L, and the aluminum salt in the cobalt-aluminum mixed salt solution includes at least one of aluminum sulfate, aluminum nitrate, or aluminum chloride; the precipitant solution includes at least one of ammonium carbonate, ammonium bicarbonate, sodium carbonate, or sodium bicarbonate, and the concentration of the precipitant solution is 2-3 mol / L.

[0037] A cobalt-aluminum mixed salt solution and a precipitant solution are injected concurrently into the reaction substrate. The injection flow rate of the cobalt-aluminum mixed salt solution is 25-40 mL / h, and the injection flow rate of the precipitant solution is 45-60 mL / h. The first coprecipitation reaction is carried out by controlling the reaction temperature of the first coprecipitation reaction at 43-47℃, the stirring rate at 300-350 rpm, and the pH value at 6.7-7.8, so as to achieve the first target particle size of 10-15 μm.

[0038] The co-current injection flow rates of the cobalt-aluminum mixed salt solution and the precipitant solution are reduced, the reaction temperature is lowered, and the pH value is increased to carry out a second coprecipitation reaction. In the second coprecipitation reaction, the injection flow rate of the cobalt-aluminum mixed salt solution is 8-12 mL / h, and the injection flow rate of the precipitant solution is 12-20 mL / h. The reaction temperature of the second coprecipitation reaction is 38-42℃, the stirring rate is 200-230 rpm, and the pH value is 6.8-7.5, resulting in high-aluminum uniformly doped large-particle cobalt carbonate with a particle size of 20-23 μm.

[0039] The preparation method of this invention uses a cobalt-aluminum mixed salt solution and a precipitant solution with the required concentration ratio. A first co-precipitation reaction is performed to achieve a first target particle size of 10-15 μm. Then, the co-flow rate of the cobalt-aluminum mixed salt solution and the precipitant solution is reduced, and the reaction temperature is lowered, thus reducing the reactivity of the second co-precipitation reaction. This achieves the phase transition from blocky primary particles to lamellar primary particles, which is beneficial for the adhesion and accumulation of lamellar primary particles and avoids small particle bursts. This results in high-aluminum uniformly doped large-particle cobalt carbonate with a particle size of 20-23 μm. The preparation method of this invention can effectively and stably generate large-particle cobalt carbonate with uniform particle size, good sphericity, and uniform aluminum element distribution. Furthermore, using the high-aluminum uniformly doped large-particle cobalt carbonate prepared by this invention as a precursor for preparing lithium cobalt oxide cathode materials can not only improve the electrical performance of the cathode material under high voltage but also reduce the time of the subsequent calcination process, improve efficiency, and save energy costs for mass production.

[0040] A second objective of this invention is to provide a high-alumina uniformly doped large-particle cobalt carbonate, wherein the high-alumina uniformly doped large-particle cobalt carbonate is prepared by the preparation method described in one objective.

[0041] The third objective of this invention is to provide an application of high-alumina uniformly doped large-particle cobalt carbonate, which is calcined to obtain cobalt tetroxide, which is then mixed with a lithium source and sintered to obtain lithium cobalt oxide cathode material.

[0042] The high-alumina uniformly doped large-particle cobalt carbonate is prepared by the preparation method described in one of the objectives, or the high-alumina uniformly doped large-particle cobalt carbonate is the high-alumina uniformly doped large-particle cobalt carbonate described in the second objective.

[0043] Compared with existing technical solutions, the present invention has at least the following beneficial effects:

[0044] (1) The preparation method described in this invention is based on the co-precipitation method. First, a first co-precipitation reaction is carried out to achieve a first target particle size of 10-15 μm. Then, the co-flow rate of the cobalt-aluminum mixed salt solution and the precipitant solution is reduced, and the reaction temperature is lowered, so that the reactivity of the second co-precipitation reaction is reduced, realizing the phase transformation of blocky primary particles into lamellar primary particles. This is beneficial to the adhesion and accumulation of lamellar primary particles and avoids the explosion of small particles. Thus, high-aluminum uniformly doped large particles of cobalt carbonate with a particle size of 20-23 μm can be obtained. Since the concentration of the cobalt-aluminum mixed salt solution and the precipitant solution remains unchanged, the aluminum concentration of the entire cobalt carbonate particles is uniform.

[0045] (2) Using the high-alumina uniformly doped large-particle cobalt carbonate prepared in this invention to prepare lithium cobalt oxide cathode material can not only improve the electrical performance of the cathode material under high voltage, but also reduce the time of the later calcination process, improve efficiency, and save energy costs for mass production. Attached Figure Description

[0046] Figure 1 This is an EDS cross-sectional image of Al obtained from the high-aluminum uniformly doped large-particle cobalt carbonate prepared in Example 1;

[0047] Figure 2 This is a SEM image of the high-alumina uniformly doped large-particle cobalt carbonate prepared in Example 1;

[0048] Figure 3 This is an EDS profile of Al against a uniformly doped large-particle cobalt carbonate prepared in Example 2.

[0049] Figure 4 This is a SEM image of the high-alumina uniformly doped large-particle cobalt carbonate prepared in Example 2;

[0050] Figure 5 This is an EDS cross-sectional image of Al obtained from the high-aluminum uniformly doped large-particle cobalt carbonate prepared in Example 3;

[0051] Figure 6 This is a SEM image of the high-alumina uniformly doped large-particle cobalt carbonate prepared in Example 3;

[0052] Figure 7 This is an EDS cross-sectional image of Al obtained from the high-aluminum uniformly doped large-particle cobalt carbonate prepared in Example 4;

[0053] Figure 8 This is a SEM image of the high-alumina uniformly doped large-particle cobalt carbonate prepared in Example 4;

[0054] Figure 9 This is an EDS profile of cobalt carbonate prepared in Comparative Example 1 against Al.

[0055] Figure 10 This is a SEM image of the cobalt carbonate prepared in Comparative Example 1;

[0056] Figure 11 This is the cross-sectional EDS image of cobalt carbonate prepared in Comparative Example 2 against Al.

[0057] Figure 12 This is a SEM image of the cobalt carbonate prepared in Comparative Example 2. Detailed Implementation

[0058] The technical solution of the present invention will be further described below with reference to the accompanying drawings and specific embodiments.

[0059] To better illustrate the present invention and facilitate understanding of its technical solutions, typical but non-limiting embodiments of the present invention are as follows:

[0060] Example 1

[0061] This embodiment provides a method for preparing high-alumina uniformly doped large-particle cobalt carbonate, the method comprising the following steps:

[0062] A cobalt-aluminum mixed salt solution was prepared using cobalt chloride and cobalt sulfate, wherein the cobalt concentration in the cobalt-aluminum mixed salt solution was 1.866 mol / L and the aluminum concentration was 86 mmol / L; a precipitant solution was prepared using ammonium bicarbonate, wherein the concentration of the precipitant solution was 2.78 mol / L.

[0063] A cobalt-aluminum mixed salt solution and a precipitant solution were injected concurrently into the reaction substrate. The injection flow rate of the cobalt-aluminum mixed salt solution was 30 mL / h, and the injection flow rate of the precipitant solution was 60 mL / h. The first coprecipitation reaction was carried out by controlling the reaction temperature of the first coprecipitation reaction at 45°C, the stirring rate at 350 rpm, and the pH value at 7.5-7.8, so as to achieve the first target particle size of 15 μm.

[0064] Reduce the injection flow rate of the cobalt-aluminum mixed salt solution to 10 mL / h, the injection flow rate of the precipitant solution to 18 mL / h, the reaction temperature to 42℃, the pH value to 7.2-7.5, and the stirring speed to 230 rpm to carry out the second coprecipitation reaction. After the target particle size of 21.5 μm is reached, stop feeding.

[0065] The reaction solution was fed into a centrifuge and washed sequentially with ammonium bicarbonate solution and hot water as washing media. The washed material was then dried in an oven at 100°C to finally obtain high-alumina uniformly doped large-particle cobalt carbonate with a particle size of 21.5 μm.

[0066] Figure 1 The EDS cross-sectional image of high-aluminum uniformly doped large-particle cobalt carbonate prepared in this embodiment against Al is shown. It can be seen that the aluminum element is generally uniformly distributed, but the distribution is not uniform in some places. Figure 2 The SEM image of the high-alumina uniformly doped large-particle cobalt carbonate prepared in this embodiment is shown. It can be seen that the sphericity is good and the particle size distribution is relatively uniform.

[0067] Example 2

[0068] This embodiment provides a method for preparing high-alumina uniformly doped large-particle cobalt carbonate, the method comprising the following steps:

[0069] A cobalt-aluminum mixed salt solution was prepared using cobalt chloride and cobalt sulfate, wherein the cobalt concentration in the cobalt-aluminum mixed salt solution was 1.866 mol / L and the aluminum concentration was 58 mmol / L; a precipitant solution was prepared using ammonium bicarbonate, wherein the concentration of the precipitant solution was 2.78 mol / L.

[0070] A cobalt-aluminum mixed salt solution and a precipitant solution were injected concurrently into the reaction substrate. The injection flow rate of the cobalt-aluminum mixed salt solution was 25 mL / h, and the injection flow rate of the precipitant solution was 45 mL / h. The first coprecipitation reaction was carried out by controlling the reaction temperature of the first coprecipitation reaction at 43°C, the stirring rate at 300 rpm, and the pH value at 7.0-7.5, so as to achieve the first target particle size of 15 μm.

[0071] Reduce the injection flow rate of the cobalt-aluminum mixed salt solution to 8 mL / h, the injection flow rate of the precipitant solution to 12 mL / h, the reaction temperature to 40℃, the pH value to 6.8-7.0, and the stirring speed to 210 rpm to carry out the second coprecipitation reaction. After the target particle size of 21.5 μm is reached, stop feeding.

[0072] The reaction solution was fed into a centrifuge and washed sequentially with ammonium bicarbonate solution and hot water as washing media. The washed material was then dried in an oven at 110°C to finally obtain high-alumina uniformly doped large-particle cobalt carbonate with a particle size of 21.5 μm.

[0073] Figure 3 The EDS cross-sectional image of high-aluminum uniformly doped large-particle cobalt carbonate prepared in this embodiment against Al is shown. It can be seen that the aluminum element distribution is not very uniform. Figure 4 The SEM image of the high-alumina uniformly doped large-particle cobalt carbonate prepared in this embodiment is shown. It can be seen that the sphericity is good and the particle size distribution is relatively uniform.

[0074] Example 3

[0075] This embodiment provides a method for preparing high-alumina uniformly doped large-particle cobalt carbonate, the method comprising the following steps:

[0076] A cobalt-aluminum mixed salt solution was prepared using cobalt chloride and cobalt sulfate, wherein the cobalt concentration in the cobalt-aluminum mixed salt solution was 1.866 mol / L and the aluminum concentration was 114 mmol / L; a precipitant solution was prepared using ammonium bicarbonate, wherein the concentration of the precipitant solution was 2.78 mol / L.

[0077] A cobalt-aluminum mixed salt solution and a precipitant solution were injected concurrently into the reaction substrate. The injection flow rate of the cobalt-aluminum mixed salt solution was 40 mL / h, and the injection flow rate of the precipitant solution was 60 mL / h. The first coprecipitation reaction was carried out by controlling the reaction temperature of the first coprecipitation reaction at 45°C, the stirring rate at 350 rpm, and the pH value at 6.7-7.0, so as to achieve the first target particle size of 15 μm.

[0078] Reduce the injection flow rate of the cobalt-aluminum mixed salt solution to 12 mL / h, reduce the injection flow rate of the precipitant solution to 19.2 mL / h, reduce the reaction temperature to 40℃, raise the pH value to 7.0-7.3, reduce the stirring speed to 200 rpm, carry out the second coprecipitation reaction, and stop feeding after the target particle size of 21.5 μm is reached.

[0079] The reaction solution was fed into a centrifuge and washed sequentially with ammonium bicarbonate solution and hot water as washing media. The washed material was then dried in an oven at 120°C to finally obtain high-alumina uniformly doped large-particle cobalt carbonate with a particle size of 21.5 μm.

[0080] Figure 5 The EDS cross-sectional image of high-aluminum uniformly doped large-particle cobalt carbonate prepared in this embodiment with respect to Al is shown. It can be seen that the aluminum element is uniformly distributed. Figure 6 The SEM image of the high-alumina uniformly doped large-particle cobalt carbonate prepared in this embodiment is shown. It can be seen that the sphericity is good and the particle size distribution is relatively uniform.

[0081] Example 4

[0082] This embodiment provides a method for preparing high-alumina uniformly doped large-particle cobalt carbonate. Compared with Example 3, the only difference is that the pH value of the first coprecipitation reaction is 7.0-7.3, while the pH value of the second coprecipitation reaction is 6.7-7.0, that is, the pH value is reduced.

[0083] Figure 7 The cross-sectional EDS image of high-aluminum uniformly doped large-particle cobalt carbonate prepared in this embodiment against Al is shown. It can be seen that the aluminum element is generally uniformly distributed, but the distribution is not uniform in some places, and there are bright spots in the aluminum distribution. Figure 8The SEM image of the high-alumina uniformly doped large-particle cobalt carbonate prepared in this embodiment is shown. It can be seen that the sphericity is good and there are slight small particles precipitated on the surface.

[0084] Comparative Example 1

[0085] This comparative example provides a method for preparing cobalt carbonate. The only difference from Example 3 is that the second coprecipitation reaction begins when the first target particle size reaches 7 μm.

[0086] Figure 9 The cross-sectional EDS image of cobalt carbonate prepared in this comparative example against Al is shown, which shows that the Al distribution is not uniform. Figure 10 The SEM image of the cobalt carbonate prepared in this comparative example is shown. It can be seen that the surface of the cobalt carbonate particles is smooth, but there are many small particles.

[0087] Comparative Example 2

[0088] This comparative example provides a method for preparing cobalt carbonate. The only difference from Example 3 is that the second coprecipitation reaction is only started after the first target particle size reaches 17 μm.

[0089] Figure 11 The cross-sectional EDS image of cobalt carbonate prepared in this comparative example against Al is shown, which shows that the Al distribution is not uniform. Figure 12 The SEM image of the cobalt carbonate prepared in this comparative example is shown. It can be seen that the surface of the cobalt carbonate particles is porous.

[0090] In summary, the preparation method of this invention is based on a co-precipitation method. First, a first co-precipitation reaction is carried out to achieve a first target particle size of 10-15 μm. Then, the co-flow rate of the cobalt-aluminum mixed salt solution and the precipitant solution is reduced, and the reaction temperature is lowered, which reduces the reactivity of the second co-precipitation reaction. This achieves the phase transition from blocky primary particles to lamellar primary particles, which is beneficial to the adhesion and accumulation of lamellar primary particles and avoids the bursting of small particles. As a result, high-aluminum uniformly doped large-particle cobalt carbonate with a particle size of 20-23 μm can be obtained. Since the concentrations of the cobalt-aluminum mixed salt solution and the precipitant solution remain unchanged, the aluminum concentration of the entire cobalt carbonate particle is uniform.

[0091] The present invention has been illustrated with the above embodiments to illustrate its detailed structural features. However, the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvements to the present invention, equivalent substitutions for the components used in the present invention, additions of auxiliary components, and selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

[0092] The preferred embodiments of the present invention have been described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the scope of the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention, and these simple modifications all fall within the protection scope of the present invention.

[0093] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction. In order to avoid unnecessary repetition, the present invention will not describe the various possible combinations separately.

[0094] Furthermore, various different embodiments of the present invention can be combined in any way, as long as they do not violate the spirit of the present invention, they should also be regarded as the content disclosed by the present invention.

Claims

1. A method for preparing high-alumina uniformly doped large-particle cobalt carbonate, characterized in that, The preparation method includes the following steps: A cobalt-aluminum mixed salt solution and a precipitant solution are injected concurrently into the reaction substrate to carry out the first coprecipitation reaction. After the first target particle size of 10-15 μm is achieved, the concurrent injection flow rate of the cobalt-aluminum mixed salt solution and the precipitant solution is reduced, the reaction temperature is lowered, and a second coprecipitation reaction is carried out to obtain high-aluminum uniformly doped large-particle cobalt carbonate with a particle size of 20-23 μm. The pH value of the first coprecipitation reaction is lower than the pH value of the second coprecipitation reaction; In the first coprecipitation reaction, the injection flow rate of the cobalt-aluminum mixed salt solution is 25-40 mL / h, and the injection flow rate of the precipitant solution is 45-60 mL / h; the reaction temperature of the first coprecipitation reaction is 43-47℃; and the pH value of the first coprecipitation reaction is 6.7-7.

0. In the second coprecipitation reaction, the injection flow rate of the cobalt-aluminum mixed salt solution is 8-12 mL / h, and the injection flow rate of the precipitant solution is 12-20 mL / h; the reaction temperature of the second coprecipitation reaction is 38-42℃; and the pH value of the second coprecipitation reaction is 7.1-7.

5.

2. The preparation method according to claim 1, characterized in that, The cobalt concentration in the cobalt-aluminum mixed salt solution is 1.8-2 mol / L.

3. The preparation method according to claim 1, characterized in that, The cobalt salt in the cobalt-aluminum mixed salt solution includes at least one of cobalt sulfate, cobalt nitrate, or cobalt chloride.

4. The preparation method according to claim 1, characterized in that, The aluminum concentration in the cobalt-aluminum mixed salt solution is 57-115 mmol / L.

5. The preparation method according to claim 1, characterized in that, The aluminum salt in the cobalt-aluminum mixed salt solution includes at least one of aluminum sulfate, aluminum nitrate, or aluminum chloride.

6. The preparation method according to claim 1, characterized in that, The precipitant solution includes at least one of ammonium carbonate, ammonium bicarbonate, sodium carbonate, or sodium bicarbonate.

7. The preparation method according to claim 1, characterized in that, The concentration of the precipitant solution is 2-3 mol / L.

8. The preparation method according to claim 1, characterized in that, The stirring rate for the first coprecipitation reaction is 300-350 rpm.

9. The preparation method according to claim 1, characterized in that, The stirring rate for the second coprecipitation reaction is 200-230 rpm.

10. A high-alumina uniformly doped cobalt carbonate with large particles, characterized in that, The high-alumina uniformly doped large-particle cobalt carbonate is prepared by the preparation method described in any one of claims 1-9.

11. An application of high-alumina uniformly doped large-particle cobalt carbonate, characterized in that, High-alumina uniformly doped cobalt carbonate particles are calcined, and the resulting cobalt tetroxide is mixed with a lithium source and then sintered to obtain lithium cobalt oxide cathode material. The high-alumina uniformly doped large-particle cobalt carbonate is prepared by the preparation method described in any one of claims 1-9, or the high-alumina uniformly doped large-particle cobalt carbonate is the high-alumina uniformly doped large-particle cobalt carbonate described in claim 10.

Citation Information

Patent Citations

  • Preparation method of large-particle-size and high-density spherical cobalt oxide

    CN105399148A

  • Preparation method of large-particle-size aluminum-doped cobalt trioxide

    CN108649219A

  • Aluminum-doped cobaltosic oxide core-shell material and preparation method thereof

    CN112723422A

  • Aluminum-doped cobalt carbonate, aluminum-doped cobaltosic oxide and preparation method and application thereof

    CN118183869A