Molten salt modifiers for modified SiO2 oxides, their preparation methods and applications
By treating the cracked region of SiCf/SiC ceramic matrix composites with a molten salt modifier consisting of Ca-based alkaline oxides and low-melting-point inorganic salts, CaSiO₃ is generated, and the SiO₂ oxide film is removed using an acid pickling solution. This solves the problem of removing harmful SiO₂ oxides from cracks in SiCf/SiC ceramic matrix composites after service, thus improving the repair quality and performance.
Patent Information
- Application Number
- CN202410447251.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-15
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-04-15
Smart Images

Figure CN118515504B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of advanced weldable ceramic matrix composites, specifically relating to a molten salt modifier and its preparation method, as well as its application in the treatment of harmful SiO2 oxides generated in the crack region of modified SiCf / SiC ceramic matrix composites in aero-engines after service. Background Technology
[0002] SiCf / SiC ceramic matrix composites are a type of composite material made by combining SiC ceramics as the matrix with SiCf fibers. They possess outstanding characteristics such as high temperature resistance, wear resistance, corrosion resistance, high-temperature creep resistance, low thermal conductivity, low coefficient of thermal expansion, and wave absorption capabilities, making them one of the most promising materials for next-generation aero-engines. It is generally believed that when the thrust-to-weight ratio of an engine reaches or exceeds 15, ceramic matrix composites are necessary to ensure engine performance meets standards. The high-temperature components of aero-engines mainly include the combustion chamber, high / low-pressure turbine guide vanes, rotor blades, and turbine outer rings. Previously, these components primarily used high-temperature alloys, with a temperature limit maintained at around 1100℃. Now, the application of SiCf / SiC ceramic matrix composites has increased the engine's temperature resistance to 1200–1350℃. Furthermore, the mass of ceramic matrix composite components is typically one-third to one-quarter of the mass of high-temperature alloy components, achieving not only engine weight reduction but also improved fuel economy.
[0003] Because SiCf / SiC ceramic matrix composites are typically used in extreme environments with complex loads such as oxygen, high temperature, and high pressure, crack damage is inevitable. In practical engineering applications, due to the high cost of SiCf / SiC ceramic matrix composites, it is often necessary to repair and reuse ceramic matrix composite components that have developed cracks after service. However, the area near cracks in SiCf / SiC ceramic matrix composites is often accompanied by severe oxidation, with a large amount of harmful SiO2 oxide film present. During the repair process, a good interfacial reaction between the repair material and the matrix material is a prerequisite for achieving performance restoration after repair. However, the SiO2 oxide film formed at the crack damage site is difficult to wet and react with inactive repair materials, which seriously affects the joint performance. At the same time, when there is an incompletely removed SiO2 oxide film at the crack, the repair material and the matrix will not fully fuse, resulting in inclusions and porosity defects, ultimately affecting the repair quality. Currently, the main cleaning method for removing oxide films near cracks in high-temperature alloys is fluoride ion cleaning technology. At temperatures above 800°C, hydrogen fluoride reacts with all oxides, carbides, nitrides, and carbon to form fluorides and water. This method can remove oxide scale without damaging the metal alloy matrix material. However, this method is not applicable to SiCf / SiC ceramic matrix composite systems. This is because both the SiC matrix / fiber and harmful SiO2 oxides are basic oxides with similar chemical properties. When cleaning the SiO2 oxide film formed near the ceramic matrix composite, hydrogen fluoride can also react with the SiCf fibers and the SiC filler material, leading to severe damage to the SiCf / SiC ceramic matrix composite. Therefore, for the repair of crack damage in SiCf / SiC ceramic matrix composites, research on the modification / removal of the SiO2 oxide film is essential and an effective measure to ensure the safe use of SiCf / SiC ceramic matrix composites in aero-engines.
[0004] Molten salt modification systems utilize low-melting-point molten salts as the reaction medium, enabling modification reactions of target products at lower temperatures. This effectively reduces the reaction temperature and avoids damage to component structures under high-temperature and harsh environments. In particular, the liquid environment allows for more uniform mixing of the matrix and solute, resulting in a more complete modification reaction. Chinese patent application number 201911134012.2 employs a molten salt system to obtain ultra-high temperature ZrC ceramic-modified C / C composite materials through a melt infiltration reaction. The melt infiltrated powder consists of Zr-Si mixed powder, K2ZrF6 powder, and alkali metal salts, significantly improving the ablation resistance of the C / C composite material. Chinese patent application number 202211423446.6 reports a method for preparing sulfur-modified porous carbon materials using a molten salt process. This method involves grinding and heating a mixed salt of sodium chloride, potassium chloride, and aluminum chloride to form a molten salt with a low eutectic point. Sulfur powder and porous carbon materials are then added. This preparation method induces elemental sulfur molecules to bind to unsaturated active sites on the carbon material surface, effectively locking in elemental sulfur and resulting in sulfur-modified porous carbon materials with excellent mercury ion adsorption capacity. However, there are few reports on using a molten salt modification system to modify / remove SiO2 oxide films generated at cracks in SiCf / SiC ceramic matrix composites after service life. Summary of the Invention
[0005] The purpose of this application is to provide a molten salt modifier and its preparation method for modifying harmful SiO2 oxides generated in the crack region of SiCf / SiC ceramic matrix composites in aero-engines after service, aiming to solve the shortcomings of existing technologies for removing harmful SiO2 oxides generated in the crack region of SiCf / SiC ceramic matrix composites in aero-engines after service.
[0006] The molten salt modifier provided by this invention is a highly efficient and green modified SiO2 oxide molten salt that can be mass-produced, is low in cost, has a simple process, and can efficiently repair cracks in SiCf / SiC ceramic matrix composite parts.
[0007] To achieve the above-mentioned objectives, the technical solution adopted in this application is as follows:
[0008] In a first aspect, the present invention provides a molten salt modifier comprising 0.1 to 60 wt% of a Ca-based basic oxide as a modifier and a low-melting-point inorganic salt as a flux.
[0009] The molten salt modifier contains, by weight percentage, 45-90% inorganic salt and 10-55% Ca-based basic oxide.
[0010] The Ca-based basic oxide is selected from at least one of CaCO3, CaO, or Ca(OH)2.
[0011] The inorganic salt is selected from at least one of KCl, NaCl, LiCl or CaCl2.
[0012] Secondly, the present invention provides a method for preparing the above-mentioned molten salt modifier, comprising the following steps: directly mixing a Ca-based basic oxide with an inorganic salt.
[0013] Thirdly, the present invention provides the application of the above-mentioned molten salt modifier in removing and / or modifying SiO2 oxide generated in the crack region after service of SiCf / SiC ceramic matrix composites.
[0014] In the aforementioned application, the removal and / or modification method includes the following steps: ball milling Ca-based alkaline oxides and inorganic salts into powder, and then, under an inert atmosphere, placing SiCf / SiC ceramic matrix composite parts with SiO2 oxide at the cracks after service into the ball-milled powder for molten salt modification treatment.
[0015] Fourthly, the present invention provides a method for using the above-mentioned molten salt modifier to remove and / or modify SiO2 oxides generated in the crack region of SiCf / SiC ceramic matrix composite material after service, comprising the following steps: ball milling Ca-based alkaline oxide and inorganic salt into powder, and then, under an inert atmosphere, treating the SiCf / SiC ceramic matrix composite material parts with SiO2 oxides in the crack region after service with molten salt in the ball-milled powder.
[0016] In the removal and / or modification method, the ball milling speed is 100–500 r / min, and the ball milling time is 30 min–10 h.
[0017] In the removal and / or modification method, the molten salt modification heating temperature is 500–1100℃, and the holding time is 30–300 min.
[0018] In the removal and / or modification method, the inert atmosphere is selected from N2 or Ar gas.
[0019] In the removal and / or modification method, the heating rate before molten salt modification is 1-5 °C / min.
[0020] The removal and / or modification method further includes acid washing of the SiCf / SiC ceramic matrix composite parts after molten salt modification.
[0021] Preferably, the acid solution is selected from at least one of hydrochloric acid, sulfuric acid, or nitric acid solution.
[0022] Beneficial Effects: This invention provides a molten salt modifier for modifying harmful SiO2 oxides generated in the crack region of SiCf / SiC ceramic matrix composites in aero-engines after service. The molten salt system fully utilizes the characteristic that Ca-based alkaline oxide molten salts can react with SiO2 oxides inside the cracks of SiCf / SiC ceramic matrix composites to generate CaSiO3 oxides, but do not react with alkaline oxide SiCf fibers and the SiC matrix. This effectively alters the chemical properties of the SiO2 oxide film. Subsequently, an acid pickling solution is used to react with the modified alkaline oxide CaSiO3, ultimately achieving the effect of removing the harmful SiO2 oxide film from the cracks.
[0023] The molten salt system used in this invention alters the properties of SiO2 oxide. Because it is a contact-type chemical reaction, the reaction process is not limited by the structure, size, or tooling of the components. Furthermore, the melting point of this molten salt system can be effectively controlled by adjusting the proportion of inorganic salts added, depending on the temperature tolerance of the components. Attached Figure Description
[0024] Figure 1 This is a SEM image of the cracks and SiO2 oxide film formed at the crack sites of the SiCf / SiC ceramic matrix composite material after high-temperature service in Example 1 of the present invention.
[0025] Figure 2 This is a SEM image of the SiO2 oxide film generated at the crack site after high-temperature service of the SiCf / SiC ceramic matrix composite material modified with molten salt modifier (molten salt system) in Example 1 of the present invention.
[0026] Figure 3 The bending results are shown for the SiO2 oxide film generated at the cracks of SiCf / SiC ceramic matrix composite parts after high-temperature service without cleaning, and for the repair after cleaning the SiO2 oxide film generated at the cracks of SiCf / SiC ceramic matrix composite parts after high-temperature service using the molten salt system of Example 1. Detailed Implementation
[0027] To make the technical problems, solutions, and beneficial effects of this application clearer, the following detailed description is provided in conjunction with the embodiments. Unless otherwise defined, all technical terms used herein have the same meaning as understood by one of ordinary skill in the art.
[0028] To efficiently remove or modify harmful SiO2 oxides generated in the crack region of SiCf / SiC ceramic matrix composites in aero-engines after service, while ensuring no damage to the SiCf / SiC ceramic matrix composite matrix material, this invention provides a molten salt modifier for modifying harmful SiO2 oxides generated in the crack region of SiCf / SiC ceramic matrix composites in aero-engines after service. The modifier comprises 0.1–60 wt% of a Ca-based basic oxide as a modifier and a low-melting-point inorganic salt as a flux.
[0029] The molten salt of this invention is similar to an aqueous solution. Molten salt is a high-temperature flux that does not contain water. Its main characteristic is that it dissociates into ions when it melts. Positive and negative ions interact with each other through Coulomb forces, so it can be used as a reaction medium at high temperatures.
[0030] In one specific embodiment of the present invention, the molten salt modifier contains 45-90% inorganic salt and 10-55% Ca-based basic oxide by mass percentage.
[0031] This invention utilizes a high-temperature chemical reaction between Ca-based basic oxides and SiO2 to generate CaSiO3, thereby removing SiO2 formed on the surface of SiC objects due to high-temperature oxidation. Ca-based basic oxides generally have high melting points; excessive amounts can raise the reaction temperature, causing thermal corrosion of the remaining SiC and reducing its lifespan. Conversely, low amounts may result in incomplete reaction with SiO2, and also slow down the reaction, increasing its reaction time. Therefore, the molten salt modifier in this invention uses 0.1–60 wt% Ca-based basic oxides. Further, it uses 45–90% inorganic salts and 10–55% Ca-based basic oxides.
[0032] In one specific embodiment of the present invention, the Ca-based basic oxide is selected from at least one of CaCO3, CaO, or Ca(OH)2.
[0033] In one specific embodiment of the present invention, the inorganic salt is selected from at least one of KCl, NaCl, LiCl or CaCl2.
[0034] This invention uses low-melting-point inorganic salts because their low melting point allows the chemical modification of Ca-based basic oxides and SiO2 to proceed at low temperatures. The melting point can also be controlled by adjusting the amount of inorganic salt added. Furthermore, when selecting specific low-melting-point inorganic salts, it is essential to ensure that they do not react with the SiC matrix or with Ca-based basic oxides. Therefore, the inorganic salt is preferably selected from at least one of KCl, NaCl, LiCl, or CaCl2.
[0035] In one embodiment of the present invention, the present invention provides a method for preparing the above-mentioned molten salt modifier, comprising the following steps: directly mixing Ca-based basic oxides with inorganic salts.
[0036] In one embodiment of the present invention, the present invention provides the application of the above-mentioned molten salt modifier in removing and / or modifying SiO2 oxide generated in the crack region after service of SiCf / SiC ceramic matrix composites.
[0037] In one embodiment of the present invention, the present invention provides a method for using the above-mentioned molten salt modifier to remove and / or modify SiO2 oxides generated in the crack region after the SiCf / SiC ceramic matrix composite material has been in service.
[0038] In one specific embodiment of the present invention, the removal and / or modification method includes the following steps: ball milling Ca-based alkaline oxides and inorganic salts into powder, and then, under an inert atmosphere, molten salt modification treatment of SiCf / SiC ceramic matrix composite parts with SiO2 oxide at the cracks after service in the ball-milled powder.
[0039] In one specific embodiment of the present invention, in the removal and / or modification method, the ball milling speed is 100-500 r / min and the ball milling time is 30 min-10 h.
[0040] In one specific embodiment of the present invention, in the removal and / or modification method, the molten salt modification heating temperature is 500-1100℃, and the holding time is 30-300min.
[0041] In one specific embodiment of the present invention, in the removal and / or modification method, the inert atmosphere is selected from N2 or Ar gas.
[0042] In one specific embodiment of the present invention, in the removal and / or modification method, the heating rate before molten salt modification heating is 1-5°C / min.
[0043] In one specific embodiment of the present invention, the removal and / or modification method further includes acid washing the SiCf / SiC ceramic matrix composite parts after molten salt modification. Preferably, the acid solution is selected from at least one of hydrochloric acid, sulfuric acid, or nitric acid solution.
[0044] The present invention requires that the molten salt modifier be used to remove and / or modify the SiO2 oxide generated in the crack region of SiCf / SiC ceramic matrix composite after service in an inert atmosphere. This is because the removed SiO2 is generated on the surface of SiC due to the reaction of SiC with oxygen. In order to avoid secondary oxidation of the SiC surface, it is necessary to choose to react under an inert gas condition.
[0045] In the removal and / or modification method, the Ca-based basic oxide and inorganic salt are first mixed uniformly by mechanical ball milling. Further heating the molten salt to a high temperature of 500–1100°C ensures that the Ca-based basic oxide is fully melted and reacts with SiO2. Controlling the reaction time to 30–300 min ensures the Ca-based basic oxide reacts fully with SiO2, achieving complete removal of SiO2. Using an inert atmosphere for SiO2 removal prevents secondary oxidation of the SiC matrix, generating harmful SiO2 phases. Simultaneously, the heating rate must be controlled at a moderate rate of 1–5°C / min. Excessive heating may cause excessive thermal stress within the molten salt, leading to expansion and sputtering, while excessively slow heating may prolong the reaction cycle and reduce production efficiency.
[0046] The following specific embodiments will be provided to explain the solution of the present invention. Those skilled in the art will understand that the following embodiments are for illustrative purposes only and should not be considered as limiting the scope of the invention. Where specific techniques or conditions are not specified in the embodiments, they are performed according to the techniques or conditions described in the literature in the field or according to the product instructions. Reagents or instruments whose manufacturers are not specified are all conventional products that can be obtained commercially.
[0047] Example 1: Modified SiCf / SiC ceramic matrix composite turbine outer ring simulates harmful SiO2 oxides at crack sites after service of components.
[0048] 1) Use a high-energy ball mill to ball mill 10% CaCO3, 45% KCl and 45% NaCl by weight, with a ball-to-material mass ratio of 25:1, a ball milling speed of 350 r / min and a ball milling time of 4 hours to obtain uniform powder.
[0049] 2) Combine the powder obtained in step 1) with SiCf / SiC parts that have developed cracks after service (e.g., Figure 1 As shown, the microstructure of cracked SiCf / SiC parts after service exhibits a significant harmful Si oxide phase. The parts were placed in a temperature-controlled tube furnace under a nitrogen atmosphere, heated at a rate of 5°C / min to 1100°C, held for 1 hour, and then allowed to cool naturally to room temperature. At this point, the SiO2 oxide scale at the cracks in the SiCf / SiC parts after service transformed into CaSiO3. Next, deionized water was used to clean the salt near the SiCf / SiC parts.
[0050] 3) Place the SiCf / SiC parts obtained in step 2) in 500 mL of 3M HCl solution, maintain the temperature at 45℃, and keep it at this temperature for 12 hours. Then, clean the SiCf / SiC parts with deionized water. Figure 2As shown, only the fibrous structure is displayed at the crack, which means that the SiO2 impurities at the crack were successfully removed after service.
[0051] 4) Further select SiCf / SiC parts with similar transverse and longitudinal crack dimensions after service. Select one part to undergo the aforementioned molten salt system method for cleaning the SiO2 harmful phase at the crack site; select another part to leave it untreated. Further repair the cracks in both parts using brazing, and test the bending performance of the repaired parts. The results are as follows: Figure 3 As shown in the figure, it is clear that the bending performance of SiCf / SiC parts with cracks cleaned by molten salt is about twice that of parts without treatment of the harmful SiO2 phase at the crack. This means that after molten salt cleaning, the harmful SiO2 phase at the crack of SiCf / SiC parts will effectively improve the repair performance of SiCf / SiC parts.
[0052] Example 2: Modified SiCf / SiC ceramic matrix composite high-conductivity blade simulates harmful SiO2 oxides at crack sites after service.
[0053] 1) Use a high-energy ball mill to ball mill 12% Ca(OH)2, 30% KCl and 58% NaCl by weight. The mass ratio of ball to material is 25:1. The ball milling speed is 350 r / min and the ball milling time is 4 hours to obtain uniform powder.
[0054] 2) Place the powder obtained in step 1) and the serviced SiCf / SiC parts in a temperature-controlled tube furnace. Under a nitrogen atmosphere, heat at a rate of 5°C / min until reaching 1100°C, hold for 1 hour, and then allow to cool naturally to room temperature. At this point, the SiO2 oxide scale at the cracks in the SiCf / SiC parts after service will transform into CaSiO3. Next, use deionized water to clean the salt near the SiCf / SiC parts.
[0055] 3) Place the SiCf / SiC parts obtained in step 2) in 500 mL of 3M HCl and 2M HNO3 solution, maintain the temperature at 45℃, and keep it at this temperature for 12 hours. Then, clean the SiCf / SiC parts with deionized water. Finally, clean parts with SiO2 oxide scale removed from the cracks are obtained.
[0056] It should be noted that the specific features, structures, materials, or characteristics described in this specification may be combined in any suitable manner in one or more embodiments. Furthermore, those skilled in the art can combine and integrate the different embodiments described in this specification and the features of those embodiments without contradiction.
Claims
1. A method for using molten salt modifiers to remove and / or modify SiO2 oxides generated in crack regions of SiCf / SiC ceramic matrix composites after service, characterized in that: Includes the following steps: Ca-based alkaline oxides and low-melting-point inorganic salts are ball-milled into powder. Under an inert atmosphere, SiCf / SiC ceramic matrix composite parts with SiO2 oxide at the cracks after service are placed in the ball-milled powder for molten salt modification treatment. The SiCf / SiC ceramic matrix composite parts after molten salt modification are then acid-washed. The molten salt of Ca-based alkaline oxides reacts with the oxide SiO2 inside the cracks of the SiCf / SiC ceramic matrix composite to generate oxide CaSiO3, but does not react with the alkaline oxide SiCf fibers and SiC matrix. The molten salt modifier contains, by weight percentage, 45-90% low-melting-point inorganic salt and 10-12% Ca-based basic oxide; the Ca-based basic oxide is selected from at least one of CaCO3 and Ca(OH)2; the low-melting-point inorganic salt is selected from at least one of KCl and NaCl; The heating temperature for molten salt modification is 1100℃; The heat preservation time is 1 hour; The heating rate before molten salt modification was 5℃ / min.
2. The method of use according to claim 1, characterized in that: Meet at least one of the following: The ball mill speed is 100–500 r / min; The ball milling time is 30 min to 10 h; The inert atmosphere is selected from N2 or Ar gas.
3. The method of use according to claim 2, characterized in that: The acid solution is selected from at least one of hydrochloric acid, sulfuric acid, or nitric acid solution.
Citation Information
Patent Citations
Preparation method of ultrahigh-temperature ceramic modified C / C composite material
CN110803942A
Preparation method of sulfur-modified porous material by molten salt method and its application
CN115739018B
Method of desilicicating coal ash deeply and recovering silicon resource
CN112077116A