A method for producing a sintering flux for protecting a furnace
By mixing waste magnesia-chrome bricks with blast furnace gas ash to form pellets, which are then used as slag splashing furnace protection modifiers, the problems of blast furnace gas ash treatment and the resource utilization of waste magnesia-chrome bricks have been solved, improving the slag splashing furnace protection effect and reducing the temperature and iron consumption of converter slag.
Patent Information
- Application Number
- CN202410473471.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-19
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-04-19
AI Technical Summary
There is no effective process in the current technology to fully process blast furnace gas ash, and the direct dumping of waste magnesia-chrome bricks will cause environmental harm. At the same time, there is a lack of effective ways to utilize magnesia-chrome bricks as resources.
Waste magnesia-chrome bricks are mixed with blast furnace gas ash in a certain proportion, pressed into pellets, and used as a slag splashing furnace protection modifier. Resource utilization is achieved through chemical reaction, and the converter slag splashing furnace protection process is optimized.
It has enabled the resource utilization of waste magnesia-chrome bricks and blast furnace gas ash, improved the effect of slag splashing and furnace protection, reduced the temperature and iron consumption of converter slag, and reduced processing costs.
Abstract
Description
Technical Field
[0001] This invention relates to a method for producing a slag splashing furnace protection modifier. Background Technology
[0002] Magnesia-chrome spinel bricks possess advantages such as high high-temperature strength, excellent thermal shock stability, strong resistance to alkaline slag erosion, and some adaptability to acidic slags, making them widely used in lime and cement production. However, discarded magnesia-chrome bricks contain toxic chromium (Cr). 6+ Ions, if directly dumped into the environment without treatment, are harmful to the environment. According to literature (1), Zhang Dandan, Li Zhijian and others published a paper entitled "Experimental Study on the Production of Magnesium-chrome Bricks from Recycled Waste Magnesium-chrome Bricks" in the second issue of the journal "Silicate Bulletin" in 2014. The article contains the statement that “magnesia-chrome bricks produced from waste magnesia-chrome bricks can replace directly bonded magnesia-chrome bricks and be used in thermal equipment such as cement rotary kilns, non-ferrous metal smelting and reburning magnesia vertical kilns.” (2) Zhang Jingyu, Sun Jialin and others published a paper entitled “Application Research of Waste Magnesia-chrome Bricks in Magnesia Spraying Material” in the second issue of Metallurgical Energy magazine in 2007. The paper contains the statement that “magnesia spraying material was produced using waste magnesia-chrome bricks from Baosteel RH with chemical composition (mass fraction): MgO 66.75%, CaO 1.25%, SiO2 1.51%, Fe2O3 6.82%, Cr2O3 19.61%. The performance indicators all reached the indicators of pure magnesia spraying material RP1 and RP2, and satisfactory results were achieved in field application.” The above literature does not mention the process method of producing converter slag splashing furnace protector modifier using waste magnesia-chrome bricks.
[0003] Blast furnace gas ash is a product obtained through wet dust removal, resulting from particulate matter generated during blast furnace smelting along with raw material dust carried by blast furnace gas and from intense reactions in the high-temperature zone. As a byproduct of the iron and steel industry, blast furnace gas ash is primarily composed of iron and carbon, with an iron content of approximately 30% and a carbon content of approximately 20%. Additionally, because some blast furnaces use iron ore containing a certain amount of non-ferrous metals, some low-boiling-point non-ferrous metals volatilize within the blast furnace and enter the blast furnace gas, ultimately accumulating in the gas sludge as oxides.
[0004] .
[0005] The resource utilization processes for blast furnace gas ash involve rotary hearth and vertical shaft furnaces. After removing zinc, lead, potassium, and sodium from the gas ash, the remaining iron-containing pellets are returned to the ironmaking process for resource utilization. Apart from this, there is currently no effective process method that can efficiently process all blast furnace gas ash.
[0006] According to literature (1), Liu Bingguo, Peng Jinhui, Zhang Libo, et al. published a paper entitled "Research Status of Resource Recycling of Blast Furnace Gas Sludge (Ash)" in the 5th issue of Mining Express in 2007. The paper states that "In 1976, the U.S. Environmental Protection Agency (EPA) enacted a law classifying lead-zinc-containing steel plant dust as K061 substances (toxic solid waste)." The content states that lead, zinc, etc., must be recycled or passivated, otherwise they must be sealed and stored in a designated area. (2) Jia Guoli and Zhang Binghuai published a paper entitled "Research on Mixed Injection of Blast Furnace Gas Ash and Pulverized Coal" in the 5th issue of "China Metallurgy" in 2007. The paper states that "Blast furnace gas ash is one of the by-products produced in the blast furnace smelting process, which contains a large amount of beneficial iron and carbon. At present, some foreign steel companies use landfill to treat it, while domestic companies basically adopt the treatment method of returning it to sintering and re-agglomerating. Mixing it with pulverized coal and injecting it into the blast furnace through the tuyeres is a technology with great development potential for utilizing blast furnace gas ash. Mixed injection can not only effectively utilize the useful substances in the ash, but also achieve the purpose of reducing the coke ratio, increasing output, and facilitating the stable and smooth operation of the furnace."
[0007] As can be seen from the above description, there is currently no process for producing slag splashing furnace protection modifiers using blast furnace gas ash. Summary of the Invention
[0008] The purpose of this invention is to provide a production method for a slag splashing furnace protection modifier, which improves the effect of slag splashing furnace protection while making resource-efficient use of waste magnesia-chromium spinel bricks and blast furnace gas ash, resulting in significant economic and environmental benefits.
[0009] The technical solution adopted in this invention is a production method of a slag splashing furnace protection modifier, which is implemented according to the following steps: 1) Crush the waste magnesia-chrome bricks to between 1mm and 5mm and transport them to the pelletizing production line for later use; 2) Blast furnace gas ash is transported to the pelletizing production line for later use, wherein the TC in the blast furnace gas ash is greater than 20% by mass. 3) The above-mentioned waste magnesia-chrome bricks and blast furnace gas ash are mixed at a mass percentage ratio of 65:35, and then pressed into 30-50mm pellets on a high-pressure dry powder briquetting machine, and transported to the converter production line for use; the main components of the slag splashing furnace protection modifier are: Cr2O3>10%, C>6%, all by mass percentage; 4) After the converter taps steel, it is in the smelting position. The above pellets are added as a slag splashing furnace protection modifier: the amount of pellets added is 3.5-5 kg per ton of steel. Then the converter is operated according to the traditional slag splashing furnace protection operation. High-pressure nitrogen is blown in to implement the slag splashing furnace protection process.
[0010] This invention uses a crusher to crush waste magnesia-chrome bricks to between 1mm and 5mm, adds some blast furnace gas ash to form pellets, and then uses them in the slag splashing furnace protection modification process. This optimizes the converter slag splashing furnace protection process while making resource utilization of two types of solid waste.
[0011] The innovations of this invention are as follows: 1) The inventors discovered that adding waste magnesia-chrome bricks to converter slag increases the viscosity of the slag, making it a high-melting-point suspended substance that can improve the foaming of converter slag, thus shortening the slag-raising time; 2) The inventors were the first in the industry to discover the mineral structure of magnesia-chrome spinel, which can combine with the reaction layer of the furnace lining magnesia-carbon bricks to form a stable network structure, reducing the shedding of the slag splashing layer and helping to maintain the slag splashing protection effect; 3) To reduce the slag temperature of converter slag and shorten the slag splashing protection time, the inventors used blast furnace gas ash as a foaming material for converter slag during the reforming process. The coke powder in the gas ash was used as the gas source material for the formation of foam slag. At the same time, the zinc and lead elements in the blast furnace gas ash undergo a reduction reaction in the strong oxidizing converter slag and are deposited in the converter, entering the molten iron and steel in the next smelting, thus realizing the resource utilization of harmful substances in the gas ash. 4) Magnesite and raw dolomite are used as modifying materials to promote the formation of foamy slag in converter slag. The CO2 produced by the decomposition of carbonates promotes the foaming of converter slag. The converter slag splashing and furnace protection modifier produced by this invention is different from the modification principle of using magnesite and raw dolomite as modifying materials. That is, this invention uses CO bubbles generated by chemical reaction as the gas source for the formation of foamy slag in converter slag, which is beneficial to degrading TFe in slag and reducing iron consumption in the steelmaking process.
[0012] In summary, the beneficial effects of this invention are as follows: Magnesia-chromium waste refractory materials are harmful to the environment; this invention enables the full resource utilization of waste magnesia-chromium refractory materials, maximizing the potential value of solid waste. This project uses a chemical reaction between blast furnace gas ash and converter slag to lower the temperature of the converter slag, reducing TFe in the converter slag, and achieving a better slag splashing protection effect than traditional slag splashing protection processes. The slag splashing protection process can also absorb some of the blast furnace gas ash generated in the ironmaking production line, reducing the treatment cost of blast furnace gas ash. Implementation
[0013] This invention uses a 1 million-ton long-process converter steelmaking production line as an example. This converter production line is equipped with a supporting lime production line, which produces 3,000 tons of waste magnesia-chrome bricks annually. Simultaneously, the ironmaking process of this production line generates over 30 tons of blast furnace gas ash daily. The process parameters for slag splashing protection in the converter are: the tapping temperature during converter smelting is 1630℃, the converter slag temperature is between 1680 and 1780℃, and the slag splashing protection time does not exceed 3 minutes.
[0014] A method for producing a slag-splashing furnace protection modifier is carried out according to the following steps: 1) Crush the waste magnesia-chrome bricks to between 1mm and 5mm and transport them to the pelletizing production line for later use; 2) Blast furnace gas ash is transported to the pelletizing production line for later use, wherein the TC in the blast furnace gas ash is greater than 20% by mass. 3) The above-mentioned waste magnesia-chrome bricks and blast furnace gas ash are mixed at a mass percentage ratio of 65:35, and then pressed into 30-50mm pellets on a high-pressure dry powder briquetting machine, and transported to the converter production line for use; the main components of the slag splashing furnace protection modifier are: Cr2O3>10%, C>6%, all by mass percentage; 4) After the converter taps steel, it is in the smelting position. The above pellets are added as a slag splashing furnace protection modifier: the amount of pellets added is 3.5-5 kg per ton of steel. Then the converter is operated according to the traditional slag splashing furnace protection operation. High-pressure nitrogen is blown in to implement the slag splashing furnace protection process.
Claims
1. A method for producing a slag-splashing furnace protection modifier, characterized in that... Follow these steps: 1) Crush the waste magnesia-chrome bricks to between 1mm and 5mm and transport them to the pelletizing production line for later use; 2) Blast furnace gas ash is transported to the pelletizing production line for later use, wherein the TC in the blast furnace gas ash is greater than 20% by mass. 3) The above-mentioned waste magnesia-chrome bricks and blast furnace gas ash are mixed at a mass percentage ratio of 65:35, and then pressed into 30-50mm pellets on a high-pressure dry powder briquetting machine, and transported to the converter production line for use; the main components of the slag splashing furnace protection modifier are: Cr2O3>10%, C>6%, all by mass percentage; 4) After the converter taps steel, it is in the smelting position. The above pellets are added as a slag splashing furnace protection modifier: the amount of pellets added is 3.5-5 kg per ton of steel. Then the converter is operated according to the traditional slag splashing furnace protection operation. High-pressure nitrogen is blown in to implement the slag splashing furnace protection process.
Citation Information
Patent Citations
Method for converter production and blast furnace gas ash resource utilization
CN115786696A
Method for recycling magnesium-containing mixed waste brick slag
CN116854492A