High-purity aluminum-silicon-copper target material, preparation method and application thereof

By employing a multi-directional forging process, alternating longitudinal and transverse cold rolling, solution treatment, and C-scan detection, the problems of uneven precipitate distribution and grain size in aluminum-silicon-copper alloy targets were solved, thereby improving the quality and performance of the targets and films.

CN118516627BActive Publication Date: 2026-11-24GUIYAN ADVANCED NEW MATERIALS (SHANGHAI) CO LTD +2
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410555866.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-07
Publication Date
2026-11-24
Estimated Expiration
2044-05-07

AI Technical Summary

Technical Problem

Existing technologies cannot ensure the uniform dispersion of precipitated phases and the uniform and fine grain size of aluminum-silicon-copper alloy targets, which affects the performance and application effect of sputtered films.

Method used

By employing a multi-directional forging and alternating longitudinal and transverse cold rolling plastic deformation process, combined with solution treatment and C-scan detection, and through repeated plastic deformation and heat treatment in each direction, the uniformity of the internal structure of aluminum-silicon-copper and defect detection are ensured, thus obtaining high-purity aluminum-silicon-copper sputtering targets.

Benefits of technology

It improves the sputtering performance of aluminum-silicon-copper targets and the performance of sputtered thin films, and reduces resource waste and defect rate in the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118516627B_ABST
    Figure CN118516627B_ABST
Patent Text Reader

Abstract

This invention discloses a high-purity aluminum-silicon-copper sputtering target, its preparation method, and its application, belonging to the technical field of sputtering targets for integrated circuit interconnects. The preparation method includes: S1: homogenization annealing; S2: multi-directional forging; S3: first C-scan inspection; S4: solution treatment; S5: alternating longitudinal and transverse cold rolling; S6: second C-scan inspection; S7: recrystallization annealing; S8: roughing, bonding, finishing, surface treatment, and cleaning. Through multi-directional forging and alternating longitudinal and transverse cold rolling, the directionality of forging and rolling is clearly defined. Repeated plastic deformation in each direction makes the internal structure of the high-purity aluminum-silicon-copper more uniformly stressed, resulting in better grain refinement. Solution treatment ensures that the precipitated phases inside the high-purity aluminum-silicon-copper are dispersed. C-scan inspection provides a more comprehensive assessment of the billet, ensuring that the final high-purity aluminum-silicon-copper sputtering target has a high yield rate and improving the quality of the final prepared sputtering target.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of sputtering target technology for integrated circuit interconnects, and relates to a high-purity aluminum-silicon-copper target, its preparation method and application. Background Technology

[0002] With the rapid development of semiconductor integrated circuits and the increase in chip integration, metal interconnects are also showing a trend towards being thinner, narrower, and more delicate. High-purity aluminum sputtering targets, as one of the main source materials for metal interconnects (usually in thin film form) in integrated circuit manufacturing, occupy a large market share due to their excellent electrical conductivity, thermal conductivity, corrosion resistance, and cost advantages.

[0003] High-purity aluminum-silicon-copper alloy thin films are usually deposited on silicon wafers. Because silicon is added to the original aluminum thin film process, it can prevent silicon elements in the silicon wafer from diffusing into the aluminum film, causing aluminum and silicon to dissolve and form spikes, which would lead to film failure. At the same time, the addition of copper to the aluminum film can improve resistance to electromigration, which ultimately makes the aluminum-silicon-copper alloy thin film stand out among many aluminum alloy thin films.

[0004] Aluminum-silicon-copper alloy sputtering targets are crucial raw materials for preparing aluminum-silicon-copper alloy thin films. The uniformity of the multi-scale microstructure of the target directly affects the uniformity of the microstructure of the sputtered film. Aluminum-silicon-copper alloy sputtering targets are alloys containing a large number of precipitates, and the proportion and distribution of these precipitates directly influence the proportion and distribution of precipitates in the sputtered film, thus affecting its subsequent performance. Simultaneously, the uniformity and fineness of the multi-scale grain size of the target directly affect the sputtering efficiency and the compositional and performance uniformity of the sputtered film. Therefore, ensuring a uniform and dispersed distribution of precipitates and uniform and fine grain size at both the macroscopic and microscopic scales is key to improving the quality of aluminum-silicon-copper alloy sputtering targets and is of great significance.

[0005] Therefore, it is necessary to provide a high-purity aluminum-silicon-copper sputtering target, its preparation method, and its application. By preparing a high-purity aluminum-silicon-copper sputtering target with uniformly dispersed precipitates and small grain size, the sputtering performance of the aluminum-silicon-copper sputtering target can be improved, thereby enhancing the performance of aluminum-silicon-copper thin films in large-scale integrated circuit interconnects. Summary of the Invention

[0006] To overcome the problems in the prior art, this invention utilizes multi-directional forging and alternating longitudinal and transverse cold rolling to clearly define the directionality of forging and rolling. Through repeated plastic deformation in each direction, the internal structure of high-purity aluminum-silicon-copper is subjected to more uniform stress, resulting in better grain refinement. Solution treatment ensures that the precipitated phases within the high-purity aluminum-silicon-copper are dispersed. Furthermore, C-scan detection provides a more comprehensive assessment of the billet, ensuring that only qualified billets proceed to subsequent processes. This guarantees that the final high-purity aluminum-silicon-copper target material has a high yield rate, reducing resource waste during preparation and improving the quality of the final high-purity aluminum-silicon-copper target material.

[0007] Furthermore, the technical problem to be solved by the present invention includes:

[0008] (1) The large plastic deformation process of multi-directional forging + alternating longitudinal and transverse rolling is adopted. Multi-directional forging forces the billet to be affected by large plastic deformation in all directions. Tensile stress and compressive stress are applied to the billet alternately, so that the grains are relatively uniformly broken. At the same time, alternating longitudinal and transverse rolling is adopted to ensure that the billet is subjected to balanced forces in the longitudinal and transverse directions, so that billets with similar grain breakage can be obtained, ensuring the relative uniformity of microstructure during plastic deformation.

[0009] (2) C-scan inspection: When the billet surface quality is good and there are no defects, ultrasonic non-destructive C-scan inspection is performed, and the bottom wave image of the billet is analyzed in combination with the flaw wave image. If the flaw wave image shows no internal defects, the bottom wave image can better reflect the attenuation degree of the billet itself: if the bottom wave attenuation is obvious, it indicates that there are more grain boundaries; if the bottom wave attenuation is not obvious, it indicates that there are fewer grain boundaries. According to the bottom wave image, the uniformity of the microstructure of the billet can be observed from the macroscopic scale. By inspecting the flaw wave image and bottom wave image of the billet after multi-directional forging and alternating longitudinal and transverse rolling, the internal structure uniformity of the billet after each step of large deformation is strictly controlled in order to obtain a final target billet with uniform grain size on the macroscopic scale.

[0010] (3) By adopting the integrated technology of large plastic deformation + C-scan detection + heat treatment, through the coordinated cooperation of large plastic deformation and heat treatment processes, and the assistance of C-scan detection, high-purity aluminum-silicon-copper targets with dispersed precipitate distribution, uniform and fine grain size and no internal defects such as pores, cracks, and delamination can be obtained.

[0011] To achieve the above objectives, the present invention is implemented through the following technical solution:

[0012] This invention provides a method for preparing a high-purity aluminum-silicon-copper target, the method comprising the following steps:

[0013] S1: Homogenization annealing: After holding the cylindrical high-purity aluminum-silicon copper ingot at 450-550℃ for 2-12 hours, it is subjected to water quenching to obtain high-purity aluminum-silicon copper billet.

[0014] S2: Multi-directional forging: Taking any radial direction of the cylindrical high-purity aluminum-silicon copper billet obtained in step S1 as the X direction, the radial direction perpendicular to the X direction as the Y direction, and the height direction of the cylindrical high-purity aluminum-silicon copper billet as the Z direction; firstly, the billet is preheated, then forged along the Z direction at a forging ratio of 2-4, then forged along the X direction at a forging ratio of 2-2.5, and finally forged along the Y direction at a forging ratio of 2-3, and the above forging process is repeated at least twice. After forging, it is water-cooled to obtain a square aluminum-silicon copper billet;

[0015] S3: First C-scan inspection: Perform C-scan inspection on the high-purity aluminum-silicon-copper billet after water cooling in step S2. Use the bottom wave diagram to determine whether the uniformity of the grain size inside the billet is qualified; use the flaw wave diagram to determine whether there are defects inside the billet. If the uniformity of the grain size inside the billet is not qualified or there are defects inside the billet, it is determined to be unqualified. The unqualified billet is reworked to step S2 for multi-directional forging again, and then C-scan inspection is performed again. If it is qualified, proceed to the next step. If it is still unqualified after 3 reworks, it is scrapped directly.

[0016] S4: Solution treatment: The square high-purity aluminum-silicon copper billet that passed the test in step S3 is kept at 400-500℃ for 4-10 hours and then subjected to water quenching.

[0017] S5: Alternating longitudinal and transverse cold rolling: First, longitudinal cold rolling is performed along the Y direction of the square high-purity aluminum-silicon-copper billet, and then transverse cold rolling is performed along the X direction of the high-purity aluminum-silicon-copper billet. The above rolling process is repeated at least 6 times, with a total rolling deformation of 65%-90%. After rolling, the billet is water-cooled.

[0018] S6: Secondary C-scan inspection: The high-purity aluminum-silicon-copper billet rolled in step S5 is leveled and then subjected to C-scan inspection. The uniformity of the internal grain size of the billet is determined by the bottom wave pattern; the presence of defects inside the billet is determined by the flaw wave pattern. If the uniformity of the internal grain size of the billet is not qualified or there are defects inside the billet, it is determined to be unqualified, and the unqualified billet is directly scrapped.

[0019] S7: Recrystallization annealing: The qualified high-purity aluminum-silicon copper billet obtained in step S6 is kept at 360-460℃ for 1-8 hours and then subjected to water quenching.

[0020] S8: After the high-purity aluminum-silicon-copper billet after water quenching in step S7 is subjected to roughing, bonding, fine machining, surface treatment and cleaning in sequence, a high-purity aluminum-silicon-copper target material is obtained.

[0021] Preferably, in step S2, the preheating temperature is 100-200℃.

[0022] Preferably, the preheating time is 20-60 minutes.

[0023] Preferably, the specific method for C-scan detection of grain size uniformity inside the billet in steps S3 and S6 is as follows: Two to three points are arbitrarily selected along the thickness direction of the billet, and the thickness L is measured using a micrometer. The C-scan device measures the propagation time t of the ultrasonic wave at that point in the billet and calculates the sound velocity C at that point. 材 The specific calculation is as follows: Among them, C 材 Let be the material's sound velocity, t be the propagation time along the billet thickness, and L be the billet thickness. Then, the intrinsic sound velocity of the billet is obtained by averaging the sound velocities at multiple points on the billet. Next, 3-5 arbitrary points on the billet are selected, and the gain height of the bottom wave peak is adjusted to between 80% and 90%. A C-scan is then performed to obtain the bottom wave map. The color differences in the bottom wave map reflect the differences in grain size within the billet.

[0024] Preferably, the method for determining whether the uniformity of the billet grain size is qualified is as follows: the bottom wave image is processed by software to exclude the edge effect area after the billet is imaged, and its average value and standard deviation are calculated. In the first C-scan detection, if the standard deviation is ≤25 and the color distribution of the bottom wave image is uniform, the uniformity of the internal grain size of the billet is qualified. In the second C-scan detection, if the standard deviation is ≤10 and the color distribution is uniform, the uniformity of the internal grain size of the billet is qualified.

[0025] Preferably, in steps S3 and S6, when C-scan detects internal defects in the billet, the gain is increased by 10-15dB to the bottom wave gain.

[0026] Preferably, in step S6, the high-purity aluminum-silicon-copper billet is leveled, and the flatness is ≤0.3mm.

[0027] Preferably, the aluminum-silicon-copper ingot has a purity ≥5N5, wherein the silicon content is 0.9-1.1wt% and the copper content is 0.4-0.6wt%.

[0028] In another aspect, the present invention obtains a high-purity aluminum-silicon-copper target material through preparation, wherein the precipitated phase of the high-purity aluminum-silicon-copper target material is dispersedly distributed and the grain size is uniform and fine.

[0029] This invention also proposes the application of this high-purity aluminum-silicon-copper target in sputtering coating of interconnects in large-scale integrated circuits.

[0030] The beneficial effects of this invention are:

[0031] 1. This invention utilizes a multi-directional forging + alternating longitudinal and transverse cold rolling process to achieve high plastic deformation. This process clearly defines the directionality of forging and rolling, and through repeated plastic deformation in each direction, effectively solves the problems of cracking and significant differences in grain fragmentation caused by uneven stress on the billet. This provides a better prerequisite for achieving uniform grain size at both the macroscopic and microscopic scales. Ultimately, the internal structure of high-purity aluminum-silicon-copper exhibits more uniform stress, better grain refinement, and an average grain size ≤100μm.

[0032] 2. This invention performs a solution treatment between multi-directional forging and alternating longitudinal and transverse cold rolling, which allows the uneven precipitates in the alloy after forging to be re-dissolved into the alloy, providing a better initial state for subsequent cold deformation treatment, and ultimately resulting in a dispersed distribution of precipitates in the high-purity aluminum-silicon-copper target material.

[0033] 3. This invention utilizes C-scan detection on high-purity aluminum-silicon-copper billets during the preparation process. By employing ultrasonic longitudinal wave pulse reflection technology and flaw wave imaging, it eliminates the influence of internal defects such as pores, cracks, and delamination on the backwave. The more grain boundaries within the billet, the more severe the scattering, leading to greater attenuation of the echo signal. Based on this principle, the distribution of grain boundaries in different locations at a macroscopic scale, i.e., grain size uniformity, can be observed through the backwave imaging. Finally, the billet is judged according to the uniformity criteria provided in this patent, improving the yield rate of high-purity aluminum-silicon-copper target materials and preventing a large number of defective products from entering subsequent processes, thus avoiding waste of preparation time and energy resources.

[0034] 4. This invention improves the performance of sputtered thin films by using high-purity aluminum-silicon-copper targets with dispersed precipitate distribution and uniform and fine grain size in sputtering coating. Attached Figure Description

[0035] Figure 1 This is a SEM image of the microstructure of the high-purity aluminum-silicon-copper target material prepared in Example 1 of this invention.

[0036] Figure 2 These are the C-scan waveform and bottom waveform during a single C-scan detection in Embodiment 1 of the present invention, wherein Figure (a) is the C-scan waveform and Figure (b) is the C-scan bottom waveform.

[0037] Figure 3 These are the C-scan waveform and bottom waveform during the secondary C-scan detection in Embodiment 1 of the present invention, wherein Figure (a) is the C-scan waveform and Figure (b) is the C-scan bottom waveform.

[0038] Figure 4 This is an elemental surface distribution diagram of the high-alumina silicon-copper target material prepared in Example 1 of the present invention.

[0039] Figure 5This is a SEM image of the microstructure of the high-purity aluminum-silicon-copper target material prepared in Example 2 of this invention.

[0040] Figure 6 These are the C-scan waveform and bottom waveform of Comparative Example 1 of this invention during a single C-scan detection. Figure (a) is the C-scan waveform, and Figure (b) is the C-scan bottom waveform.

[0041] Figure 7 This is a SEM image of the microstructure of the high-purity aluminum-silicon-copper target material prepared in Comparative Example 2 of this invention.

[0042] Figure 8 This is an elemental surface distribution diagram of the high-alumina silicon-copper target material prepared in Comparative Example 2 of this invention. Detailed Implementation

[0043] The present invention will be further described in detail below with reference to specific embodiments.

[0044] In the embodiments and comparative examples of this invention, all chemical reagents not specifically described were commercially available analytical grade reagents used in the experiments.

[0045] Example 1

[0046] Example 1 of the present invention prepares a high-purity aluminum-silicon-copper target material through the following steps:

[0047] (1) Homogenization annealing: The cylindrical high-purity aluminum-silicon copper ingot is kept at 520℃ for 12 hours and then water quenched to obtain high-purity aluminum-silicon copper billet.

[0048] (2) Multi-directional forging: First, the billet is preheated at 150℃ for 30 minutes. Taking any radial direction of the cylindrical high-purity aluminum-silicon copper billet as the X direction, the radial direction perpendicular to the X direction as the Y direction, and the height direction of the cylindrical high-purity aluminum-silicon copper billet as the Z direction, forging is first carried out along the Z direction at a forging ratio of 3, then along the X direction at a forging ratio of 2, and finally along the Y direction at a forging ratio of 2.5. The multi-directional forging is repeated twice. After forging, the billet is water-cooled to obtain a square aluminum-silicon copper billet.

[0049] (3) Single C-scan inspection: Before inspection, surface defects of the billet are removed with a milling cutter. Then, a C-scan inspection is performed on the billet. Three points are randomly selected along the thickness direction of the billet, and the intrinsic sound velocity of the billet is calculated. Subsequently, the gain height of the bottom wave peak is adjusted to 85% at any three points. At the same time, during the billet defect wave inspection, the gain of the bottom wave is increased by 10dB. The billet C-scan bottom wave diagram is shown below. Figure 2As shown in (b), excluding the edge effect area after billet imaging, the average value is 76.02, and the standard deviation is 23.05. Furthermore, the color distribution in the bottom ripple pattern is relatively uniform, indicating that the billet's microstructure is relatively uniform and the grain size uniformity is acceptable. The billet C-scan ripple pattern is as follows: Figure 2 As shown in (a), through Figure 2 (a) It can be seen that there are no defects inside the billet. Therefore, in this embodiment, the billet is judged to be qualified and proceeds to the next process.

[0050] (4) Solution treatment: The high-purity aluminum-silicon copper billet is kept at 500℃ for 8 hours and then water quenched.

[0051] (5) Alternating longitudinal and transverse cold rolling: First, the billet is cold rolled longitudinally along the Y direction, and then cold rolled transversely along the X direction. The alternating longitudinal and transverse cold rolling is repeated 6 times, with a total rolling deformation of 65%. After rolling, the billet is water-cooled.

[0052] (6) Secondary C-scan inspection: Before inspection, the billet is leveled to a flatness of ≤0.2mm; surface defects are removed with a milling cutter. The rolled billet is then subjected to C-scan inspection, using the same method as step (3). The billet C-scan bottom waveform is shown below. Figure 3 As shown in (b), excluding the edge effect area after billet imaging, the average value is 91.67, and the standard deviation is 6.55. Furthermore, the color distribution in the bottom ripple pattern is relatively uniform, indicating that the billet's microstructure is relatively uniform and the grain size uniformity is acceptable. The billet C-scan ripple pattern is as follows: Figure 3 As shown in (a), through Figure 3 (a) It can be seen that there are no defects inside the billet. Therefore, in this embodiment, the billet is judged to be qualified and proceeds to the next process.

[0053] (7) Recrystallization annealing: The high-purity aluminum-silicon copper billet is kept at 400℃ for 4 hours and then water quenched.

[0054] (8) After the high-purity aluminum-silicon-copper billet is subjected to rough processing, bonding, fine processing, surface treatment and cleaning in sequence, a high-purity aluminum-silicon-copper target material is obtained.

[0055] SEM experiments were performed on the high-purity aluminum-silicon-copper target material prepared in this embodiment, and the SEM results of the high-purity aluminum-silicon-copper target material are as follows: Figure 1 As shown.

[0056] pass Figure 1 It can be seen that the target material grains are fine and uniform, with an average grain size of approximately 50 μm. Figure 2 (a) It can be seen that the forged billet is free of defects such as porosity, inclusions, cracks, and delamination; through Figure 2 (b) It can be seen that the standard deviation of the bottom wave pattern after forging is 23.05, which is considered a qualified target billet. Through... Figure 3(a) It can be seen that the cold-rolled billet is free of defects such as porosity, inclusions, cracks, and delamination; through Figure 3 (b) It can be seen that the standard deviation of the bottom ripple pattern after cold rolling is 6.55, which indicates that the billet is qualified. Figure 4 It can be seen that the precipitated phase of the target material is mainly a Si-containing precipitate, and its distribution is relatively uniform.

[0057] Example 2

[0058] Example 2 of the present invention prepares high-purity aluminum-silicon-copper target material through the following steps:

[0059] (1) Homogenization annealing: The cylindrical high-purity aluminum-silicon copper ingot is kept at 450℃ for 10 hours and then water quenched to obtain high-purity aluminum-silicon copper billet.

[0060] (2) Multi-directional forging: First, the billet is preheated at 100℃ for 60 minutes. Taking any radial direction of the cylindrical high-purity aluminum-silicon copper billet as the X direction, the radial direction perpendicular to the X direction as the Y direction, and the height direction of the cylindrical high-purity aluminum-silicon copper billet as the Z direction, forging is first carried out along the Z direction at a forging ratio of 2, then along the X direction at a forging ratio of 2, and finally along the Y direction at a forging ratio of 3. The multi-directional forging is repeated 3 times. After forging, the billet is water-cooled to obtain a square aluminum-silicon copper billet.

[0061] (3) First C-scan inspection: Before inspection, surface defects of the billet are removed with a milling cutter. Then, a C-scan inspection is performed on the billet. Two points are randomly selected in the thickness direction of the billet, and the intrinsic sound velocity of the billet is calculated. Subsequently, five points are randomly selected and the gain height of the bottom wave peak is adjusted to 80%. At the same time, during the billet flaw wave inspection, the gain of the bottom wave is increased by 15dB. The edge effect area after the billet imaging is excluded, and its average value is 75.29, standard deviation is 24.02. The color distribution in the bottom wave image is relatively uniform, indicating that the microstructure of the billet is relatively uniform and the grain size uniformity is qualified. The flaw wave image shows that there are no defects inside the billet. Therefore, the billet in this embodiment is judged to be qualified and proceeds to the next process.

[0062] (4) Solution treatment: The high-purity aluminum-silicon copper billet is kept at 400℃ for 10 hours and then water quenched.

[0063] (5) Alternating longitudinal and transverse cold rolling: First, the billet is cold rolled longitudinally along the Y direction, then the billet is cold rolled transversely along the X direction, and the alternating longitudinal and transverse cold rolling is repeated 7 times. The total deformation of the rolling is 80%, and the billet is water-cooled after rolling.

[0064] (6) Secondary C-scan inspection: Before inspection, the billet is leveled, and its flatness is ≤0.2mm; surface defects are removed with a milling cutter. The rolled billet is subjected to C-scan inspection, and the inspection method is the same as in step (3). The edge effect area after the billet imaging is excluded, and its average value is 90.22, standard deviation is 8.91, and the color distribution in the bottom wave image is relatively uniform, indicating that the microstructure of the billet is relatively uniform and the grain size uniformity is qualified. It can be seen from the flaw wave image that there are no defects inside the billet. Therefore, the billet in this embodiment is judged to be qualified and enters the next process.

[0065] (7) Recrystallization annealing: The high-purity aluminum-silicon copper billet is kept at 460℃ for 1 hour and then water quenched.

[0066] (8) After the high-purity aluminum-silicon-copper billet is subjected to rough processing, bonding, fine processing, surface treatment and cleaning in sequence, a high-purity aluminum-silicon-copper target material is obtained.

[0067] SEM experiments were performed on the high-purity aluminum-silicon-copper target material prepared in this embodiment, and the SEM results of the high-purity aluminum-silicon-copper target material are as follows: Figure 5 As shown.

[0068] pass Figure 5 It can be seen that the grain size of the target material is small, about 80 μm, and the grain size distribution is uniform.

[0069] Example 3

[0070] Example 3 of the present invention prepares a high-purity aluminum-silicon-copper target material through the following steps:

[0071] (1) Homogenization annealing: The cylindrical high-purity aluminum-silicon copper ingot is kept at 550℃ for 2 hours and then water quenched to obtain high-purity aluminum-silicon copper billet.

[0072] (2) Multi-directional forging: First, the billet is preheated at 200℃ for 20 minutes. Taking any radial direction of the cylindrical high-purity aluminum-silicon copper billet as the X direction, the radial direction perpendicular to the X direction as the Y direction, and the height direction of the cylindrical high-purity aluminum-silicon copper billet as the Z direction, forging is first carried out along the Z direction at a forging ratio of 4, then along the X direction at a forging ratio of 2.3, and finally along the Y direction at a forging ratio of 2. The multi-directional forging is repeated 4 times. After forging, the billet is water-cooled to obtain a square aluminum-silicon copper billet.

[0073] (3) First C-scan inspection: Before inspection, surface defects of the billet are removed with a milling cutter. Then, a C-scan inspection is performed on the billet. Three points are randomly selected in the thickness direction of the billet, and the intrinsic sound velocity of the billet is calculated. Subsequently, four points are selected to adjust the gain height of the bottom wave peak to 90%. At the same time, during the billet flaw wave inspection, the gain of the bottom wave is increased by 12dB. The edge effect area after the billet imaging is excluded. The average value is 74.92, the standard deviation is 24.57, and the color distribution in the bottom wave image is relatively uniform, indicating that the microstructure of the billet is relatively uniform and the grain size uniformity is qualified. The flaw wave image shows that there are no defects inside the billet. Therefore, the billet in this embodiment is judged to be qualified and proceeds to the next process.

[0074] (4) Solution treatment: The high-purity aluminum-silicon copper billet is kept at 450℃ for 4 hours and then water quenched.

[0075] (5) Alternating longitudinal and transverse cold rolling: First, the billet is cold rolled longitudinally along the Y direction, and then cold rolled transversely along the X direction. The alternating longitudinal and transverse cold rolling is repeated 8 times, with a total rolling deformation of 90%. After rolling, the billet is water-cooled.

[0076] (6) Secondary C-scan inspection: Before inspection, the billet is leveled, and its flatness is ≤0.2mm; surface defects are removed with a milling cutter. C-scan inspection is performed on the rolled billet, and the inspection method is the same as in step (3). The edge effect area after the billet imaging is excluded, and its average value is 90.16, standard deviation is 9.14, and the color distribution in the bottom wave image is relatively uniform, indicating that the microstructure of the billet is relatively uniform and the grain size uniformity is qualified. It can be seen from the flaw wave image that there are no defects inside the billet. Therefore, the billet in this embodiment is judged to be qualified and enters the next process.

[0077] (7) Recrystallization annealing: After holding the high-purity aluminum-silicon copper billet at 360℃ for 8 hours, it is subjected to water quenching.

[0078] (8) After the high-purity aluminum-silicon-copper billet is subjected to rough processing, bonding, fine processing, surface treatment and cleaning in sequence, a high-purity aluminum-silicon-copper target material is obtained.

[0079] Comparative Example 1

[0080] Comparative Example 1 uses the same method as Example 1 to prepare high-purity aluminum-silicon-copper target material, the difference being that: this comparative example only undergoes one multi-directional forging.

[0081] The damage waveform obtained from a single C-scan scan in this comparative example is shown below. Figure 6 As shown in (a), the bottom wave diagram is as follows: Figure 6 As shown in (b). Through Figure 6 (a) It can be seen that the forged billet is free of defects such as porosity, inclusions, cracks, and delamination; through Figure 6 (b) It can be seen that the mean value of the bottom wave image after forging, excluding the edge effect area after billet imaging, is 61.55, and the standard deviation is 33.23, which is judged as an unqualified target billet.

[0082] Comparative Example 2

[0083] Comparative Example 2 uses the same method as Example 1 to prepare high-purity aluminum-silicon-copper targets, except that: no solution treatment is performed in this comparative example.

[0084] SEM experiments were performed on the high-purity aluminum-silicon-copper target material prepared in this comparative example. The SEM results of the high-purity aluminum-silicon-copper target material are as follows: Figure 7 As shown, the grain size is relatively uniform and fine, with an average grain size of 47 μm. According to... Figure 8 It can be seen that the precipitates of the target material are mainly Si-containing precipitates, but the precipitates are unevenly distributed, and coarsening of the precipitates occurs in some areas.

[0085] Comparative Example 3

[0086] Comparative Example 3 uses the same method as Example 1 to prepare high-purity aluminum-silicon-copper targets, except that: this comparative example does not perform multi-directional forging, but only forging in one direction.

[0087] Comparative Example 4

[0088] Comparative Example 4 uses the same method as Example 1 to prepare high-purity aluminum-silicon-copper targets, except that: this comparative example does not perform alternating longitudinal and transverse cold rolling, but only cold rolling in one direction.

[0089] The experimental results of Examples 1, 2, 3, Comparative Examples 1, 2, 3, and 4 of the present invention are shown in Table 1.

[0090] Table 1

[0091] Characterization parameters Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 A single C-scan examination of the injury waveform No defects No defects No defects No defects No defects No defects No defects Standard deviation of a single C-scan detection of the bottom waveform 23.05 24.02 24.57 33.23 12.02 39.54 23.31 A single C-scan test of the color uniformity of the bottom image Relatively uniform Relatively uniform Relatively uniform Uneven Relatively uniform Uneven Relatively uniform Secondary C-scan detection of damage waveform No defects No defects No defects No defects No defects Standard deviation of secondary C-scan detection of the bottom waveform 6.55 8.91 9.12 18.65 21.86 Secondary C-scan detection of color uniformity in the background image Relatively uniform Relatively uniform Relatively uniform Uneven Average grain size / μm 50.23 81.18 65.33 47.89 Grain size range / μm 21.65-81.70 37.14-98.17 22.05-116.53 22.22-83.57 Precipitated phase distribution Diffuse distribution Diffuse distribution Diffuse distribution Uneven distribution in conclusion qualified qualified qualified Unqualified Unqualified Unqualified Unqualified

[0092] As shown in Table 1, compared with Comparative Example 1, the billet in Example 1, which underwent multiple multi-directional forgings, exhibited better internal structural uniformity. In Comparative Example 1, the lack of repeated multi-directional forging resulted in limited plastic deformation and poor stress uniformity, leading to poor internal structural uniformity. Compared with Comparative Example 2, Example 1 showed better uniformity in the dispersion of precipitated phases. In Comparative Example 2, the absence of solution treatment prevented uniform dispersion of precipitated phases. Compared with Comparative Example 3, Example 1 showed better internal structural uniformity. However, Comparative Example 3, with forging only in one direction, resulted in uneven stress distribution in all directions, preventing the internal structural uniformity from meeting the required standards. Compared with Comparative Example 4, Example 1 showed better internal structural uniformity. However, Comparative Example 4, with cold rolling only in one direction, resulted in uneven stress distribution in all directions, preventing the internal structural uniformity from meeting the required standards.

[0093] In summary, the high-purity aluminum-silicon-copper target material prepared by the method of the present invention has small and uniform internal grain size, and its precipitated phase exhibits a relatively uniform dispersion distribution. This results in the sputtered film also having a uniformly dispersed precipitated phase and small and uniform grain size, thereby giving the sputtered film superior performance.

[0094] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made to it in form and detail without departing from the scope defined by the claims of the present invention.

Claims

1. A method for preparing a high-purity aluminum-silicon-copper target, characterized in that: The preparation method includes the following steps: S1: Homogenization annealing: After holding the cylindrical high-purity aluminum-silicon copper ingot at 450-550℃ for 2-12 hours, it is subjected to water quenching to obtain high-purity aluminum-silicon copper billet. S2: Multi-directional forging: Taking any radial direction of the cylindrical high-purity aluminum-silicon copper billet obtained in step S1 as the X direction, the radial direction perpendicular to the X direction as the Y direction, and the height direction of the cylindrical high-purity aluminum-silicon copper billet as the Z direction; firstly, the billet is preheated, then forged along the Z direction at a forging ratio of 2-4, then forged along the X direction at a forging ratio of 2-2.5, and finally forged along the Y direction at a forging ratio of 2-3, and the above forging process is repeated at least twice. After forging, it is water-cooled to obtain a square aluminum-silicon copper billet; S3: First C-scan inspection: Perform C-scan inspection on the high-purity aluminum-silicon-copper billet after water cooling in step S2. Use the bottom wave diagram to determine whether the uniformity of the grain size inside the billet is qualified; use the flaw wave diagram to determine whether there are defects inside the billet. If the uniformity of the grain size inside the billet is not qualified or there are defects inside the billet, it is determined to be unqualified. The unqualified billet is reworked to step S2 for multi-directional forging again, and then C-scan inspection is performed again. If it is qualified, proceed to the next step. If it is still unqualified after 3 reworks, it is scrapped directly. S4: Solution treatment: The square high-purity aluminum-silicon copper billet that passed the test in step S3 is kept at 400-500℃ for 4-10 hours and then subjected to water quenching. S5: Alternating longitudinal and transverse cold rolling: First, longitudinal cold rolling is performed along the Y direction of the square high-purity aluminum-silicon-copper billet, and then transverse cold rolling is performed along the X direction of the high-purity aluminum-silicon-copper billet. The above rolling process is repeated at least 6 times, and the total rolling deformation is 65%-90%. After rolling, water cooling is performed. S6: Secondary C-scan inspection: The high-purity aluminum-silicon-copper billet rolled in step S5 is leveled and then subjected to C-scan inspection. The uniformity of the internal grain size of the billet is determined by the bottom wave pattern; the presence of defects inside the billet is determined by the flaw wave pattern. If the uniformity of the internal grain size of the billet is not qualified or there are defects inside the billet, it is determined to be unqualified, and the unqualified billet is directly scrapped. S7: Recrystallization annealing: The qualified high-purity aluminum-silicon copper billet obtained in step S6 is kept at 360-460℃ for 1-8 hours and then subjected to water quenching. S8: After the high-purity aluminum-silicon-copper billet after water quenching in step S7 is subjected to roughing, bonding, fine machining, surface treatment and cleaning in sequence, a high-purity aluminum-silicon-copper target material is obtained. The specific method for detecting the uniformity of grain size inside the billet using C-scan in steps S3 and S6 is as follows: Two to three points are randomly selected along the thickness direction of the billet, and its thickness L is measured using a micrometer. The C-scan device measures the propagation time t of the ultrasonic wave at the selected points on the billet and calculates the sound velocity C at that point. 材 The specific calculation is as follows: , Among them, C 材 For the material's sound velocity, t The propagation time is in the thickness direction of the billet. L The billet thickness is then determined. Subsequently, the intrinsic sound velocity of the billet is obtained based on the average sound velocity at multiple points on the billet. Then, 3-5 points on the billet are selected and the gain height of the bottom wave peak is adjusted to be between 80% and 90%. After C-scan, the bottom wave map is obtained. The color difference of the bottom wave map reflects the difference in grain size inside the billet. The method for determining whether the uniformity of the billet grain size is qualified is as follows: the bottom wave image is processed by software to eliminate the edge effect area after the billet is imaged, and its average value and standard deviation are calculated. In the first C-scan detection, if the standard deviation is ≤25 and the color distribution of the bottom wave image is uniform, the uniformity of the internal grain size of the billet is qualified. In the second C-scan detection, if the standard deviation is ≤10 and the color distribution is uniform, the uniformity of the internal grain size of the billet is qualified.

2. The method for preparing a high-purity aluminum-silicon-copper target according to claim 1, characterized in that: In step S2, the preheating temperature is 100-200℃.

3. The method for preparing a high-purity aluminum-silicon-copper target according to claim 2, characterized in that: The preheating time is 20-60 minutes.

4. The method for preparing a high-purity aluminum-silicon-copper target according to claim 1, characterized in that: In steps S3 and S6, when C-scan detects internal defects in the billet, the gain is increased by 10-15dB to the bottom wave gain.

5. The method for preparing a high-purity aluminum-silicon-copper target according to claim 1, characterized in that: In step S6, the high-purity aluminum-silicon-copper billet is leveled, with a flatness of ≤0.3mm.

6. A method for preparing a high-purity aluminum-silicon-copper target according to any one of claims 1-5, characterized in that: The aluminum-silicon-copper ingot has a purity ≥5N5, wherein the silicon content is 0.9-1.1wt% and the copper content is 0.4-0.6wt%.

7. The high-purity aluminum-silicon-copper target material prepared by the method for preparing high-purity aluminum-silicon-copper target material according to claims 1-5 is characterized in that: The high-purity aluminum-silicon-copper target material has a dispersed precipitate distribution and uniform, fine grain size.

8. The high-purity aluminum-silicon-copper target material of claim 7 is used in the sputtering coating of interconnects in large-scale integrated circuits.

Citation Information

Patent Citations

  • Method for preparing aluminum alloy sputtering target material

    CN105525149A

  • Preparation method of large-size molybdenum-niobium planar target material