A blocked modified filler, a water-resistant paint, a coating, and a method of preparation
By using a high Tg value topcoat emulsion treatment and a two-step mixing method to prepare a closed-type modified filler, the problems of bubble defects and hydrophilicity in traditional polymer cement waterproof coatings were solved, achieving high-efficiency waterproofing, stain resistance, and construction efficiency.
Patent Information
- Application Number
- CN202410542720.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-30
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-04-30
AI Technical Summary
Traditional polymer cement waterproof coatings suffer from air bubble defects and high hydrophilicity during use, resulting in poor stain resistance and inadequate waterproofing effect.
A high Tg value topcoat emulsion is used to adsorb fillers, and a film-forming aid is combined with a curing reaction to prepare a closed modified filler. A waterproof coating is then prepared using a two-step mixing method to reduce the bubble rate and improve hydrophobicity. This coating is then used in conjunction with a penetrating primer.
It improves the density and stain resistance of the waterproof coating, reduces construction steps, and enhances the integrated effect of waterproofing and decoration, as well as construction efficiency.
Smart Images

Figure CN118530616B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the technical field of architectural coatings, and specifically relates to a closed modified filler, a waterproof coating, a coating layer, and a preparation method thereof. Background Technology
[0002] Polymer cement waterproof coatings consist of two components: a liquid and a powder. After thorough mixing, the polymer emulsion encapsulates the cement particles and other fillers and aggregates in the powder component. Upon application, some of the water in the emulsion evaporates, and the polymer particles dehydrate and adhere together, forming a continuous elastic film. Simultaneously, the remaining water in the emulsion hydrates and hardens with the cement in the powder component, while the inorganic cementitious materials in the powder component, along with the evaporating water from the emulsion, form an interpenetrating network of waterproof coating structure. However, traditional polymer cement waterproof coatings have the following drawbacks:
[0003] First, during use, the air in the gaps of the filler is replaced by the liquid components, generating a large number of bubbles. Moreover, there is not enough time to defoam at the construction site, resulting in pore defects in the coating.
[0004] Secondly, waterproof coatings have two binding substances: emulsion and cement. They have a low content of organic emulsion, a high content of powder, and a high degree of hydrophilicity.
[0005] Due to the above two issues, waterproof coatings on the market often suffer from poor stain resistance and inadequate waterproofing performance. Summary of the Invention
[0006] To address the aforementioned problems in the prior art, this application provides a closed modified filler, a waterproof coating, a coating layer, and a preparation method thereon to solve the above-mentioned technical problems.
[0007] According to a first aspect of the present invention, a method for preparing a blocked modified filler is provided, comprising:
[0008] S11, a high Tg value topcoat emulsion is uniformly sprayed onto the filler material being stirred to obtain an adsorbent filler, wherein the mass ratio of the filler material to the high Tg value topcoat emulsion is 1:0.1-0.2.
[0009] S12 involves continuously spraying a film-forming aid onto an adsorbent filler at a fixed temperature. Through a curing reaction, a closed-type modified filler is obtained. The mass ratio of the high Tg value topcoat emulsion to the film-forming aid is 1:0.07-0.15. The adsorbent-modified filler treated with the high Tg value topcoat emulsion improves the density and hydrophobicity of the powder surface.
[0010] In some specific embodiments, the high Tg value topcoat emulsion is an acrylic polymer emulsion with a Tg value of 45℃-70℃, and contains hydrophobic groups of fluorine or silicon. Adsorption treatment of the high Tg value topcoat emulsion reduces the porosity of the filler, lowers the rate of air bubbles introduced when the liquid and powder components are mixed, and reduces void defects in the waterproof coating. The adsorption-curing treatment of the high Tg value topcoat emulsion also improves the coating's stain resistance by altering the hydrophobicity of the filler surface.
[0011] In some specific embodiments, the film-forming aid is 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate and / or dipropylene glycol butyl ether.
[0012] In some specific embodiments, the fixed temperature is set to 40℃-60℃.
[0013] According to a second aspect of the present invention, a closed-type modified filler is provided, prepared by the method described in the first aspect. The closed-type modified filler solves problems such as the generation of numerous bubbles during the mixing of powder and liquid components, where air in the filler voids is replaced by the liquid component.
[0014] According to a third aspect of the present invention, a method for preparing a waterproof coating is provided, comprising:
[0015] S21, the sealed modified filler, cement, and water-reducing agent obtained in the second aspect are mixed and stirred evenly to obtain the powder component of the waterproof coating. The mass ratio of the sealed modified filler to cement is 1:0.05-0.18.
[0016] S22, the liquid component is divided into batches, and the powder component is added to the first batch of liquid component during stirring. After stirring evenly, component A of the waterproof coating is obtained, wherein the mass ratio of the first batch of liquid component to powder component is 1:1.8-2.2.
[0017] S23, add the remaining liquid components to component A in the stirring process, stir evenly to obtain waterproof coating, and the ratio of the total mass of liquid components to the total mass of powder components is 1:0.9-1.1.
[0018] Using a two-step or even multi-step mixing method is beneficial for powder dispersion, reduces voids in the coating, improves the stain resistance of waterproof coatings and coatings, and solves problems such as insufficient time for defoaming at the construction site, which leads to many pores and poor stain resistance in the coating.
[0019] In some specific embodiments, the liquid components include polyacrylate emulsion, titanium dioxide, sodium polyacrylate dispersant, and hydroxypropyl methylcellulose.
[0020] According to a fourth aspect of the present invention, a waterproof coating is provided, prepared by the method described in the third aspect. The waterproof coating of the present invention, through modification of the filler, avoids the problems of coatings containing both emulsion and cement as binders, having low organic emulsion content, high powder content, and high hydrophilicity of the coating.
[0021] According to a fifth aspect of the present invention, a method for preparing a waterproof coating is provided, comprising:
[0022] S31, uniformly coat a penetrating primer containing styrene-acrylate copolymer emulsion components, and dry for >4h to obtain the first coating. The dry film thickness of the penetrating primer is 10μm to 20μm.
[0023] S32, the waterproof coating obtained in the fourth aspect is applied to the upper surface of the first coating to obtain a waterproof coating, wherein the dry film thickness of the waterproof coating is 950μm to 1500μm.
[0024] According to a sixth aspect of the present invention, a waterproof coating is provided, prepared by the method described in the fifth aspect. By using the waterproof coating in conjunction with a penetrating primer, no additional topcoat is required, saving a construction layer and improving construction efficiency.
[0025] Compared with the prior art, the beneficial results of the present invention are as follows:
[0026] (1) The high Tg value topcoat emulsion is used to adsorb the filler, thereby reducing the porosity of the filler and thus reducing the bubble rate introduced when the liquid component and powder component are mixed. This ultimately reduces the defects of large and numerous voids in the waterproof coating and achieves an integrated waterproof and decorative effect.
[0027] (2) The high Tg value topcoat emulsion contains hydrophobic groups, which enhance the hydrophobicity of the sealed modified filler surface and achieve the stain resistance of the waterproof coating.
[0028] (3) The two-step mixing method of liquid component and powder component is adopted, which is conducive to powder dispersion, reduces the voids in the coating and improves the stain resistance.
[0029] (4) The waterproof coating is used in conjunction with the penetrating primer. In terms of process, there is no need to add an external topcoat, saving a construction layer and improving construction efficiency. Attached Figure Description
[0030] The accompanying drawings are included to provide a further understanding of the embodiments and are incorporated in and constitute a part of this specification. The drawings illustrate embodiments and, together with the description, serve to explain the principles of the invention. Other embodiments and many anticipated advantages of the embodiments will be readily recognized as they become better understood through reference to the following detailed description. Elements in the drawings are not necessarily to scale. The same reference numerals refer to corresponding similar parts.
[0031] Figure 1 This is a flowchart of a method for preparing a closed modified filler according to an embodiment of the present invention;
[0032] Figure 2 This is a schematic diagram of the sealing process of the sealed modified filler according to a specific embodiment of the present invention;
[0033] Figure 3 This is a flowchart of a method for preparing a waterproof coating according to an embodiment of the present invention;
[0034] Figure 4 This is a flowchart of a method for preparing a waterproof coating according to an embodiment of the present invention. Detailed Implementation
[0035] The technical solutions in the embodiments will be clearly and completely described below with reference to the accompanying drawings. Similar component reference numerals in the drawings represent similar components. Obviously, the embodiments described below are only some embodiments of the present invention, and not all embodiments. All other embodiments obtained by those skilled in the art based on the embodiments of the present invention without creative effort are within the scope of protection of the present invention.
[0036] It should be understood that, when used in this specification and the appended claims, the terms "comprising" and "including" indicate the presence of the described features, integrals, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integrals, steps, operations, elements, components and / or collections thereof.
[0037] It should also be understood that the terminology used in this specification is for the purpose of describing particular embodiments only and is not intended to limit the invention. As used in this specification and the appended claims, the singular forms “a,” “an,” and “the” are intended to include the plural forms unless the context clearly indicates otherwise.
[0038] This invention provides a method for preparing a closed modified filler, such as... Figure 1 As shown, the method includes:
[0039] S101, a high Tg value topcoat emulsion is uniformly sprayed onto the filler material being stirred to obtain an adsorbent filler material, wherein the mass ratio of the filler material to the high Tg value topcoat emulsion is 1:0.1-0.2.
[0040] S102, at a fixed temperature, film-forming aids are continuously sprayed onto adsorbent fillers, and a closed modified filler is obtained through a curing reaction. The mass ratio of high Tg value topcoat emulsion to film-forming aids is 1:0.07-0.15.
[0041] At room temperature, a high Tg value topcoat emulsion is continuously sprayed onto the filler powder while stirring. After the process is complete, a film-forming aid is continuously sprayed onto the adsorption-modified filler. The mass ratio of filler to high Tg value topcoat emulsion is 1:0.1–0.2, and the mass ratio of high Tg value topcoat emulsion to film-forming aid is 1:0.07–0.15. The temperature is set at 40–60℃, and the curing reaction time is 2–6 hours. After the reaction is completed, the sealed modified filler is obtained.
[0042] In some specific embodiments, the film-forming aid is one or more of 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate and dipropylene glycol butyl ether.
[0043] In some specific embodiments, the high Tg value cover emulsion is an acrylic polymer emulsion with a Tg of 45℃-70℃ and contains hydrophobic groups of fluorine or silicon.
[0044] In some specific embodiments, the filler is heavy calcium carbonate, wollastonite, fly ash, or one or more of these.
[0045] In a specific embodiment, refer to Figure 2 , Figure 2 A schematic diagram of the sealing process of the sealing modified filler that can be applied to embodiments of this application is shown. Figure 2 As shown, filler 1 has numerous surface pores and strong hydrophilicity. After spraying a high-Tg emulsion 2 containing hydrophobic groups and thoroughly mixing it, a film-forming aid is sprayed on to form emulsion particles 3 with adsorption properties. The emulsion particles 3 further transform into a film, forming a low-porosity and highly hydrophobic closed-loop modified filler 4 under mechanical interlocking. First, under the action of hydrogen bonds and charges on the surface of filler 1, the high-Tg emulsion 2 and film-forming aid are adsorbed and enter the surface pores. Under the condition of water evaporation, the emulsion particles 3 self-polymerize and solidify through swelling, forming a mechanical interlock between the emulsion film and the filler, while also giving the emulsion hydrophobic groups. Finally, a low-porosity, highly hydrophobic closed-loop modified filler is obtained.
[0046] This invention also proposes a method for preparing a waterproof coating, such as... Figure 3 As shown, the method includes:
[0047] S301, mix the sealed modified filler, cement, and water-reducing agent obtained in step S102, stir evenly, and obtain the powder component of the waterproof coating. The mass ratio of the sealed modified filler to cement is 1:0.05-0.18.
[0048] S302, the liquid component is divided into batches, and the powder component is added to the first batch of liquid component during stirring. After stirring evenly, component A of the waterproof coating is obtained, wherein the mass ratio of the first batch of liquid component to the powder component is 1:1.8-2.2.
[0049] S303, add the remaining liquid components to component A in the stirrer in sequence, stir evenly to obtain waterproof coating, the ratio of the total mass of liquid components to powder components is 1:0.9-1.1.
[0050] In a specific embodiment, the sealed modified filler, cement, and water-reducing agent obtained in step S102 are added to a reactor. The mass ratio of the sealed modified filler to cement is 1:0.05 to 0.18. After stirring for 10-20 minutes, the powder component of the waterproof coating is obtained.
[0051] In a specific embodiment, a portion of the liquid component is first placed in a container. Under stirring conditions, the powder component is added at a ratio of 1:1.8 to 2.2 (total mass of liquid component:total mass of powder component in container). After stirring for 15-30 minutes, the remaining liquid component is added while stirring, wherein the ratio of total mass of liquid component to total mass of powder component is 1:0.9-1.1. After stirring for 5-10 minutes, the waterproof coating is obtained.
[0052] In some specific embodiments, the main components of the liquid component are polyacrylate emulsion, titanium dioxide, sodium polyacrylate dispersant and hydroxypropyl methylcellulose, wherein the Tg value of the polyacrylate emulsion is -5℃ to 5℃.
[0053] Continue to refer to Figure 4 , Figure 4 A flowchart illustrating a method for preparing a waterproof coating applicable to embodiments of this application is shown, the method comprising:
[0054] S401, uniformly coat a penetrating primer containing styrene-acrylate copolymer emulsion components, and dry for >4h to obtain the first coating. The dry film thickness of the penetrating primer is 10μm to 20μm.
[0055] S402, the waterproof coating obtained in step S303 is applied to the upper surface of the first coating to obtain a waterproof coating, wherein the dry film thickness of the waterproof coating is 950μm to 1500μm.
[0056] In a specific embodiment, a penetrating primer is first applied, and after drying for more than 4 hours, a waterproof coating is applied to obtain a waterproof coating. The penetrating primer contains a styrene-acrylate copolymer emulsion with a particle size of 80nm to 150nm. The dry film thickness of the penetrating primer is 10μm to 20μm, and the dry film thickness of the waterproof coating is 950μm to 1500μm.
[0057] The present invention will now be further described in conjunction with specific embodiments. However, the scope of protection claimed by the present invention is not limited to the scope involved in the embodiments.
[0058] The raw materials used in the following embodiments and comparative examples are as follows:
[0059] Hydroxypropyl methylcellulose (HPMC (75,000), Shanghai Kaiyin Chemical Co., Ltd.); Sodium polyacrylate dispersant (4140, BASF Group); Cement (42.5 white cement, Alboportland (Anqing) Co., Ltd.); Wollastonite (325 mesh, Guangfu Building Materials (Jiaoling) Refined Chemical Co., Ltd.); Film-forming aid (2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, Dow Chemical); High Tg value topcoat emulsion (K-2, Dow Chemical); Polyacrylate emulsion (RS-3781, BADF Group Co., Ltd.); Titanium dioxide (R996, Longbai Xiangyang Titanium Industry Co., Ltd.); Water-reducing agent (8030, Jiangsu Zhaojia Building Materials Technology Co., Ltd.); Penetrating primer is made by adding 7% film-forming aid to RS-360 emulsion and diluting it with 50% water (RS-360, BADF Group Co., Ltd.), low Tg value emulsion, commercially available.
[0060] The stain resistance test method involves first applying a penetrating primer to the substrate, and then conducting a stain resistance test according to the specifications in GB / T9755-2014. The stain resistance (white or light-colored paint film) requirement for superior grade products in GB / T9755-2014 is ≤15%.
[0061] The following mass percentages (%) are used to illustrate the examples and comparative examples.
[0062] Example 1:
[0063] Step 1: At room temperature, based on a mass ratio of wollastonite to high Tg value topcoat emulsion of 1:0.15, the high Tg value topcoat emulsion is continuously sprayed onto the stirred filler powder (wollastonite). Then, based on a mass ratio of high Tg value topcoat emulsion to film-forming aid (2,2,4-trimethyl-1,3-pentanediol monoisobutyrate) of 1:0.1, the film-forming aid is continuously sprayed onto the adsorption-modified powder. The curing reaction is carried out at a temperature of 50°C for 4 hours. After the reaction is completed, the sealed modified filler is obtained.
[0064] The above-mentioned closed-modified filler (closed-modified wollastonite), cement, and water-reducing agent are added to the reactor, wherein the mass ratio of the closed-modified powder to the cement is 1:0.05 to 0.18. After stirring for 15 minutes, the closed-modified coating powder component is obtained.
[0065] Step two: First, place the liquid component of the waterproof coating in a container. While stirring the liquid component, add all the powder component, maintaining a liquid component to powder component ratio of 1:2. Mix thoroughly for 20 minutes, then add the remaining liquid component. After stirring for 8 minutes, the waterproof coating is ready. In this step, the ratio of the total mass of the liquid component to the total mass of the powder component is 1:(0.9-1.1).
[0066] Step 3: First, apply a penetrating primer to the substrate. After drying for 8 hours, the dry film thickness of the penetrating primer is 10μm to 20μm. Next, apply a waterproof coating on the dried penetrating primer film. The dry film thickness of the waterproof coating is 950μm to 1500μm, thus obtaining the waterproof coating.
[0067] To verify the effectiveness of the present invention, tests were conducted on the waterproof coating prepared by this method. Four sets of examples and comparative examples were prepared, and the specific proportions and test results of the four sets of examples are detailed in Table 1. The specific component details and test results of the four sets of comparative examples are detailed in Table 2. Among them, the preparation data of the closed-modified wollastonite in the four sets of examples and two sets of comparative examples are detailed in Table 3.
[0068]
[0069]
[0070] Table 1. Correspondence Table of Formulation Data for Examples
[0071] As shown in Table 1, the mass ratios of the closed-modified wollastonite to white cement in Examples 1 to 4 are 1:0.18, 1:0.05, 1:0.13, and 1:0.08, respectively. In Example 4, 7.7 kg of white cement, 92 kg of closed-modified wollastonite, and 0.3 kg of water-reducing agent were mixed and stirred for 15 minutes to obtain the powder component of the waterproof coating. The mass ratio of the closed-modified wollastonite to white cement was 1:0.08. The liquid component, with a total mass ratio of liquid component to powder component of 1:1, was processed in batches. The first batch of 50 kg of liquid component was placed in a container, and the entire 100 kg of powder component was added while stirring. After all the powder component was added, stirring continued for 20 minutes. Then, the remaining 50 kg of liquid component was added and stirred for another 8 minutes to obtain the waterproof coating with the lowest stain resistance.
[0072]
[0073]
[0074] Table 2 Comparative Example Formula Data Correspondence Table
[0075] As shown in Table 2, firstly, Comparative Example 3, which uses unmodified wollastonite as filler and does not employ two-step mixing, exhibits the worst stain resistance. Secondly, Comparative Example 1, which uses unmodified wollastonite as filler but employs two-step mixing, achieves a stain resistance of 36.3%. Next is Comparative Example 4, which uses low-Tg emulsion-modified wollastonite as filler and employs two-step mixing, achieving a stain resistance of 30%. The best stain resistance is found in Comparative Example 2, which uses modified wollastonite as filler but does not employ two-step mixing, achieving a stain resistance of 17%. Therefore, using the modified filler of this invention as part of the coating powder results in significantly better stain resistance compared to using unmodified filler or low-Tg emulsion-modified filler.
[0076] According to Tables 1 and 2, and in conjunction with Example 3 and Comparative Example 2, it can be seen that, under the same conditions, when the liquid component and powder component of the sealing and improving coating are mixed in batches, the resulting waterproof coating has better stain resistance.
[0077]
[0078] Table 3. Data correspondence of closed-modified wollastonite in the four sets of examples and two sets of comparative examples.
[0079] According to Tables 1 and 3, at room temperature, 13.8 kg of high Tg value topcoat emulsion is continuously sprayed onto 92 kg of stirred wollastonite to obtain adsorbed modified wollastonite; then, 1.5 kg of film-forming aid is continuously sprayed onto the stirred adsorbed modified wollastonite, the temperature is set at 50°C, and after curing for 4 hours, sealed modified wollastonite can be obtained; finally, the sealed modified wollastonite prepared in Example 4 of Table 3 is combined with other formulations in Example 4 of Table 1, and the above-mentioned steps are followed to prepare the waterproof coating and waterproof coating with the best stain resistance in this application.
[0080] This application discloses a closed-modified filler, a waterproof coating, a coating layer, and a preparation method. First, it utilizes an adsorption-curing treatment with a high Tg value topcoat emulsion to reduce the porosity of the filler and enhances the hydrophobicity of the filler surface through hydrophobic groups, thereby improving the surface density of the powder components. This results in a coating prepared using the closed-modified filler exhibiting superior waterproof and stain-resistant properties. Second, in the mixing and stirring of the powder components and liquid components, a two-step and multi-step mixing method is combined to achieve sufficient dispersion of the powder components, reducing voids in the coating and significantly improving the stain resistance of the waterproof coating while maintaining its waterproof function. Finally, in terms of process, the waterproof coating is used in conjunction with a penetrating primer, effectively reducing the number of application steps and improving construction efficiency while achieving waterproof and stain-resistant effects. This application solves these problems.
[0081] It is evident that those skilled in the art can make various modifications and alterations to the embodiments of the present invention without departing from the spirit and scope of the invention. In this way, the invention is also intended to cover such modifications and alterations if they fall within the scope of the claims and their equivalents. The word "comprising" does not exclude the presence of other elements or steps not listed in the claims. The simple fact that certain measures are described in mutually different dependent claims does not indicate that a combination of these measures cannot be used for profit. Any reference numerals in the claims should not be considered as limiting the scope.
Claims
1. A method for preparing a closed modified filler, characterized in that, include: S11, a high Tg value emulsion with a Tg value of 45℃-70℃ is uniformly sprayed onto the filler in a stirring process to obtain an adsorbent filler, wherein the mass ratio of the filler to the high Tg value emulsion is 1:0.1-0.2, and the high Tg value emulsion is an acrylic polymer emulsion containing hydrophobic groups of fluorine or silicon. S12, at a fixed temperature, the film-forming aid is continuously sprayed onto the adsorbent filler, and the sealed modified filler is obtained through a curing reaction. The mass ratio of the high Tg value topcoat emulsion to the film-forming aid is 1:0.07-0.15, and the film-forming aid is 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate and / or dipropylene glycol butyl ether.
2. The method for preparing the sealed modified filler according to claim 1, characterized in that, The fixed temperature is set to 40℃-60℃.
3. A type of closed-loop modified filler, characterized in that, Prepared by the method according to any one of claims 1-2.
4. A method for preparing a waterproof coating, characterized in that, include: S21, the sealing modified filler, cement, and water-reducing agent described in claim 3 are mixed and stirred evenly to obtain the powder component of the waterproof coating, wherein the mass ratio of the sealing modified filler to the cement is 1:0.05-0.18; S22, the liquid component is divided into batches, and the powder component is added to the first batch of liquid component during stirring. After stirring evenly, component A of the waterproof coating is obtained, wherein the mass ratio of the first batch of liquid component to the powder component is 1:1.8-2.
2. S23, the remaining liquid components are added to component A in the stirring process, and after stirring evenly, the waterproof coating is obtained. The ratio of the total mass of the liquid components to the total mass of the powder components is 1:0.9-1.
1.
5. The method for preparing a waterproof coating according to claim 4, characterized in that, The liquid components include polyacrylate emulsion, titanium dioxide, sodium polyacrylate dispersant, and hydroxypropyl methylcellulose.
6. A waterproof coating, characterized in that, Prepared by the method of any one of claims 4-5.
7. A method for preparing a waterproof coating, characterized in that, include: S31, uniformly coat a penetrating primer containing styrene-acrylate copolymer emulsion components, and dry for >4h to obtain a first coating layer, wherein the dry film thickness of the penetrating primer is 10μm~20μm; S32, the waterproof coating of claim 6 is applied to the upper surface of the first coating to obtain the waterproof coating, wherein the dry film thickness of the waterproof coating is 950μm to 1500μm.
8. A waterproof coating, characterized in that, It is prepared by the method described in claim 7.
Citation Information
Patent Citations
Preparation method of anti-fouling waterproof coating adopting modified acrylic acid
CN104610833A
Mildewproof and waterproof coating for building external wall and production method thereof
CN107987575A
High-density low-water-permeability water-based outer wall polymer coating material and preparation method thereof
CN113088143A
Light polymer cement waterproof coating and preparation method thereof
CN114921146A