A method for controlling quality of needle-punched nonwoven fabrics

CN118531563BInactive Publication Date: 2024-12-06ZHEJIANG SCI-TECH UNIV +2
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410994054.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure CN118531563B_ABST
    Figure CN118531563B_ABST
Patent Text Reader

Abstract

The present application relates to a method for controlling the quality of needle-punched nonwoven fabrics, wherein the method sequentially subjects the web to pre-punching treatment, main-punching treatment and cloth-surface needle-punching treatment to obtain an initial fabric, wherein the pre-punching treatment and main-punching treatment are used to adjust the web structure, and the cloth-surface needle-punching treatment is used to adjust the surface density and thickness of the web; the initial fabric is dried in a closed space by using circulating air heating, and by controlling the oven temperature of the upper and lower regions of the fabric, the drying is used to adjust the softness and hardness of the fabric; the dried fabric is surface-treated by a hot rolling roller, and the surface treatment is used to adjust the surface flatness of the fabric; the surface-treated fabric is subjected to product quality inspection, and fabrics that do not meet product quality standards are adjusted accordingly to obtain fabrics that meet product quality standards, wherein the product quality inspection includes fabric thickness, strength and elongation, gram weight, fabric softness and hardness, fabric surface flatness and metal residue rate inspection. The method realizes the control of the quality of existing needle-punched nonwoven fabrics, effectively improves the quality of nonwoven fabrics, and solves the problem of low quality of existing needle-punched nonwoven fabrics in the related technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of nonwoven fabric production, and in particular to a method for controlling the quality of needle-punched nonwoven fabrics. Background Art

[0002] Needle-punched nonwoven fabric is a type of dry-laid nonwoven fabric. It is a nonwoven fabric process that uses a needle to repeatedly puncture the fiber mesh after the fibers are loosened, combed, and laid. In recent years, the needle-punched nonwoven fabric industry has entered a period of rapid growth. Foreign advanced nonwoven fabric technology has been gradually absorbed and digested, and domestic needle-punched nonwoven fabric technology has been rapidly improved. Various new processes have emerged one after another. The successful combination of various equipment technologies and process technologies has opened up the bottlenecks that restrict production capacity, variety, and energy consumption. The product application field has been greatly broadened, which has promoted the upgrading of the overall industry.

[0003] At present, although the quality control process of needle-punched non-woven fabrics is becoming more and more perfect, due to the inadequate quality control process, the existing needle-punched non-woven fabrics have the problem of low quality. Summary of the invention

[0004] The embodiment of the present application provides a method for controlling the quality of a needle-punched nonwoven fabric, so as to at least solve the problem of low quality of the existing needle-punched nonwoven fabric in the related art.

[0005] In a first aspect, an embodiment of the present application provides a method for controlling the quality of a needle-punched nonwoven fabric, the method comprising:

[0006] The fiber web is sequentially subjected to a pre-punching treatment, a main-punching treatment and a cloth surface needle-punching treatment to obtain an initial cloth, wherein the pre-punching treatment and the main-punching treatment are used to adjust the fiber web structure, and the cloth surface needle-punching treatment is used to adjust the surface density and thickness of the fiber web;

[0007] The initial fabric is dried by heating with circulating air in a closed space and controlling the oven temperature of the upper area and the lower area of ​​the fabric, wherein the drying is used to adjust the hardness of the fabric;

[0008] The dried fabric is subjected to surface treatment by means of a hot roller, wherein the surface treatment is used to adjust the flatness of the fabric surface;

[0009] Perform product quality inspection on the surface treated fabrics, make relevant adjustments to the fabrics that do not meet the product quality standards, and obtain fabrics that meet the product quality standards, wherein the product quality inspection includes fabric thickness, strength and elongation, gram weight, fabric hardness, fabric surface smoothness and metal residue rate inspection.

[0010] In one embodiment, making relevant adjustments to fabric that does not meet product quality standards to obtain fabric that meets product quality standards includes:

[0011] When the thickness, strength, elongation and gram weight of the fabric do not meet the quality standards, the needle punching depth and needle punching density of the pre-needling treatment, the main needle punching treatment and the fabric surface needle punching treatment are adjusted;

[0012] When the hardness of the fabric does not meet the quality standard, adjusting the oven temperature of the upper area and the lower area of ​​the fabric;

[0013] When the surface flatness of the cloth does not meet the quality standard, adjusting the parameters of the surface treatment of the hot rolling roller;

[0014] In the case that the metal residue rate of the cloth does not meet the quality standard, the metal in the cloth is filtered and metal residue detection is performed on each device.

[0015] In one embodiment, the needle puncture depth of the pre-puncture treatment is 3.0-12.5 mm, and the needle puncture density of the pre-puncture treatment is 40-70 l / ㎡;

[0016] The puncture depth of the main puncture treatment is 2.5-8.0 mm, and the puncture density of the main puncture treatment is 120-200 l / ㎡;

[0017] The needle punching depth of the cloth surface needle punching treatment is 2.0-7.0 mm, and the needle punching density of the cloth surface needle punching treatment is 140-190 l / ㎡.

[0018] In one embodiment, the drying of the initial fabric by heating with circulating air in a closed space and controlling the oven temperature of the upper region and the lower region of the fabric comprises:

[0019] Gas is used for heating in a closed space, and the oven temperatures of the upper area and the lower area of ​​the cloth are controlled separately by circulating air, wherein the oven temperatures of the upper area and the lower area of ​​the cloth are controlled according to the characteristics of the cloth, the oven temperature of the upper area of ​​the cloth includes 0°C-220°C, and the oven temperature of the lower area of ​​the cloth includes 0°C-220°C.

[0020] In one embodiment, the dried fabric is subjected to surface treatment by a hot roller, and the surface treatment is used to adjust the flatness of the fabric surface, including:

[0021] Electric energy is used to circulate and heat the oil in the two hot rolling rollers, and the temperatures of the two hot rolling rollers are controlled respectively, and the upper and lower surfaces of the cloth are subjected to rolling treatment, wherein the temperature of the upper rolling roller in the hot rolling rollers includes 0℃-300℃, the temperature of the lower rolling roller in the hot rolling rollers includes 0℃-300℃, and the speed of the hot rolling rollers includes 3m / min-10m / min.

[0022] In one embodiment, before performing product quality inspection on the surface-treated fabric, the method further comprises:

[0023] The surface of the cloth is evenly powdered by a powder spreading machine.

[0024] In one embodiment, before the fiber web is subjected to a pre-needling treatment, a main needling treatment and a cloth surface needling treatment in sequence to obtain an initial cloth, the method further comprises:

[0025] Different types of fibers are fed into different bale opening machines according to the production formula, and the proportion of input materials is controlled;

[0026] The different types of fibers that pass through the bale opener are subjected to metal detection, and the raw materials after detection are initially mixed and loosened through the mixing bin;

[0027] Further mixing and finely opening the fibers after mixing in the large bin;

[0028] The mixed and opened fibers are sucked into a cotton storage box through a fan for storage and standby use.

[0029] The fibers in the cotton storage box are sent to the air pressure cotton box by a powerful fan, and the fibers are accurately weighed by a belt scale.

[0030] In one embodiment, after the fibers in the cotton storage box are sent to the air pressure cotton box by a powerful fan and the fibers are accurately weighed by a belt scale, the method further comprises:

[0031] The weighed different fibers are combed into a cross-arranged, evenly mixed single-layer fiber web through a carding machine.

[0032] In one embodiment, different weighed fibers are combed into a cross-arranged, evenly mixed single-layer fiber web by a carding machine, comprising:

[0033] A single-layer fiber web is laid out by a web laying machine into a multi-layer fiber web with a preset number of layers and uniform thickness, and the multi-layer fiber web is overlapped.

[0034] In one embodiment, after a single-layer fiber web is laid into a multi-layer fiber web having a preset number of layers and uniform thickness by a web laying machine, and the multi-layer fiber web is overlapped, the method further comprises:

[0035] The fiber web is arranged differently by changing the arrangement of the fibers through a drafting machine.

[0036] A needle-punched nonwoven fabric quality control method provided in an embodiment of the present application has at least the following technical effects.

[0037] The fiber web is subjected to pre-needling treatment, main-needling treatment and cloth surface needle-punching treatment in sequence to obtain an initial fabric, wherein the pre-needling treatment and main-needling treatment are used to adjust the fiber web structure, and the cloth surface needle-punching treatment is used to adjust the surface density and thickness of the fiber web; the initial fabric is dried by circulating air heating in a closed space and by controlling the oven temperature of the upper area and the lower area of ​​the fabric, and the drying is used to adjust the softness and hardness of the fabric; the dried fabric is surface-treated by a hot rolling roller, and the surface treatment is used to adjust the surface flatness of the fabric; the surface-treated fabric is subjected to product quality inspection, and fabrics that do not meet product quality standards are adjusted accordingly to obtain fabrics that meet product quality standards, wherein the product quality inspection includes fabric thickness, strength and elongation, gram weight, fabric softness and hardness, fabric surface flatness and metal residue rate inspection, so as to realize the control of the quality of existing needle-punched non-woven fabrics, effectively improve the quality of non-woven fabrics, and solve the problem of low quality of existing needle-punched non-woven fabrics in related technologies.

[0038] Details of one or more embodiments of the present application are set forth in the following drawings and description to make other features, objects, and advantages of the present application more readily apparent. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0040] Figure 1 It is a flow chart of the quality control of needle-punched nonwoven fabrics;

[0041] Figure 2 is a flowchart of steps S109 to S111 and step S113 according to an exemplary embodiment;

[0042] Figure 3 is a flowchart of steps S101 to S105 according to an exemplary embodiment. DETAILED DESCRIPTION

[0043] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application is described and illustrated below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. Based on the embodiments provided in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.

[0044] Obviously, the drawings described below are only some examples or embodiments of the present application. For ordinary technicians in this field, the present application can also be applied to other similar scenarios based on these drawings without creative work. In addition, it can also be understood that although the efforts made in this development process may be complicated and lengthy, for ordinary technicians in this field related to the content disclosed in this application, some changes in design, manufacturing or production based on the technical content disclosed in this application are just conventional technical means, and should not be understood as insufficient content disclosed in this application.

[0045] Reference to "embodiments" in this application means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those of ordinary skill in the art that the embodiments described in this application may be combined with other embodiments without conflict.

[0046] Unless otherwise defined, the technical terms or scientific terms involved in this application should be understood by people with ordinary skills in the technical field to which this application belongs. The words "one", "a", "a", "the" and the like involved in this application do not indicate a quantity limitation, and may indicate the singular or plural. The terms "include", "comprise", "have" and any of their variations involved in this application are intended to cover non-exclusive inclusions; for example, a process, method, system, product or device that includes a series of steps or modules (units) is not limited to the listed steps or units, but may also include steps or units that are not listed, or may also include other steps or units inherent to these processes, methods, products or devices. The words "connect", "connected", "coupled" and the like involved in this application are not limited to physical or mechanical connections, but may include electrical connections, whether direct or indirect. The "multiple" involved in this application refers to two or more. "And / or" describes the association relationship of associated objects, indicating that there may be three relationships, for example, "A and / or B" can mean: A exists alone, A and B exist at the same time, and B exists alone. The character " / " generally indicates that the objects before and after are in an "or" relationship. The terms "first", "second", "third", etc. involved in this application are only used to distinguish similar objects and do not represent a specific ordering of the objects.

[0047] At present, the production process of needle-punched non-woven fabrics mainly includes the following steps: ① Raw material preparation. Chemical fibers such as polyester and polypropylene are usually used as raw materials. ② Combing and combing. The fiber material is combed to remove impurities and make it into a continuous fiber web. ③ Pre-needling. The fiber web is preliminarily reinforced through the needle punching process. ④ Main needling. The fiber web is further reinforced through the needle punching process to form a preliminary non-woven fabric structure. ⑤ Heat setting. The non-woven fabric is heat-treated to fix its structure and increase its strength. ⑥ Surface treatment. Sometimes the surface of the non-woven fabric is treated with singeing and chemical oil to increase its smoothness and air permeability. ⑦ Rolling. After inspection, the non-woven fabric is packaged in rolls. Needle-punched nonwoven fabrics are widely used, mainly in: 1. Medical and health fields: fabrics for diapers and sanitary napkins; surgical gowns, caps, shoe covers, masks, face masks, hospital patients, bed sheets, mattresses, pillowcases, antibacterial curtains; wet towels, cotton balls, disinfection wraps; leukocyte separation materials, artificial skin; basic materials for labor protection clothing in radiation situations; medical adhesive tape base, bandage base, wound compresses, wound pads, blood-absorbing cloth. 2. Home decoration field: carpets and flooring materials; carpet base; curtains and drapes; tablecloths, bedspreads, wall coverings; mattresses, furniture covering fabrics; artificial turf. 3. Clothing field: various clothing decorative linings; winter clothing warm wadding; outerwear and underwear; clothing accessories (clothing labels, lace, bras, shoulder pads, etc.). 4. Footwear and imitation leather field: fabrics, artificial deerskin, shoes, bags, leather shoes lining; intermediate lining and support (reinforcement) materials. 5. Filter materials: Conventional filtration: used for air conditioning, kitchen smoke filters, beverage liquid filters, etc. 6. High temperature resistant and corrosion resistant filter materials: used to filter high temperature, corrosive exhaust and dust emitted by industrial furnaces. 7. Geotextiles: Geotextile infiltration ditches for underground irrigation and drainage; Geotextiles for drainage separation and reinforcement in highway and railway construction; Geotextiles for bank slope dam reinforcement; Geotextiles for bridge engineering; Waste stacking delay; Impermeable geotextiles for artificial pools; Waterproof asphalt base fabric. 8. Automobile industry: Seat covers, sun visors, soft door pads, pads and covering materials for roofs and luggage compartments, thermal insulation and sound insulation materials, vaporizers, air filter cotton, tufted carpet base fabrics, needle-punched terry-type molded carpets, sofa cushion materials. 9. Industry: Oil absorption materials for port sea surface deoiling and oil recovery in Shanghai oil production areas; Electronic insulation materials; Battery separator cloth; Industrial polishing materials; FRP pipe reinforcement substrate, industrial tape substrate, industrial hose substrate. 10. Agriculture: household harvest cloth, anti-frost curtain, anti-pest cloth, soil moisture cloth, seedling cloth, greenhouse. 11. Household products: wiping cloth, shoe cloth, suit cover, baggage cloth, bedding collection bag, pillowcase, chair sand cover, gift bag, tea bag, kitchen tea filter, water filter bag. 12. Others: disk liner; coating base cloth; packaging materials, etc.

[0048] At present, although the quality control process of needle-punched non-woven fabrics is becoming more and more perfect, due to the inadequate quality control process, the existing needle-punched non-woven fabrics have the problem of low quality.

[0049] Therefore, an embodiment of the present application proposes a needle-punched nonwoven fabric quality control method to solve the above problems.

[0050] The present application embodiment provides a method for controlling the quality of needle-punched nonwoven fabrics. Figure 1 It is a flow chart of the quality control of needle-punched nonwoven fabrics. Figure 2 is a flowchart of steps S109 to S111 and step S113 according to an exemplary embodiment. Figure 1 , Figure 2 As shown, a needle-punched nonwoven fabric quality control method includes:

[0051] Step S109, subjecting the fiber web to pre-needling treatment, main-needling treatment and surface-needling treatment in sequence to obtain an initial fabric, wherein the pre-needling treatment and main-needling treatment are used to adjust the fiber web structure, and the surface-needling treatment is used to adjust the surface density and thickness of the fiber web.

[0052] Step S110, the initial fabric is dried by heating with circulating air in a closed space and controlling the oven temperature of the upper area and the lower area of ​​the fabric, wherein the drying is used to adjust the hardness of the fabric.

[0053] Step S111: performing surface treatment on the dried cloth by means of a hot rolling roller, wherein the surface treatment is used to adjust the flatness of the cloth surface.

[0054] Step S113, performing product quality inspection on the surface treated fabric, making relevant adjustments to the fabric that does not meet the product quality standards, and obtaining fabric that meets the product quality standards, wherein the product quality inspection includes fabric thickness, strength and elongation, gram weight, fabric hardness, fabric surface flatness and metal residue rate inspection.

[0055] In summary, the embodiment of the present application provides a method for controlling the quality of needle-punched nonwoven fabrics, wherein the fiber web is subjected to pre-punching treatment, main-punching treatment and cloth surface needle-punching treatment in sequence to obtain an initial fabric, wherein the pre-punching treatment and main-punching treatment are used to adjust the fiber web structure, and the cloth surface needle-punching treatment is used to adjust the surface density and thickness of the fiber web; the initial fabric is dried in a closed space by using circulating air heating, and the oven temperature of the upper area and the lower area of ​​the fabric is controlled, and the drying is used to adjust the softness and hardness of the fabric; the dried fabric is subjected to surface treatment by a hot rolling roller, and the surface treatment is used to adjust the surface flatness of the fabric; the surface-treated fabric is subjected to product quality inspection, and fabrics that do not meet the product quality standards are adjusted accordingly to obtain fabrics that meet the product quality standards, wherein the product quality inspection includes fabric thickness, strength and elongation, gram weight, fabric softness and hardness, fabric surface flatness and metal residue rate inspection. The quality control of existing needle-punched nonwoven fabrics is achieved, the quality of nonwoven fabrics is effectively improved, and the problem of low quality of existing needle-punched nonwoven fabrics in the related art is solved.

[0056] Figure 3 is a flowchart of steps S101 to S105 according to an exemplary embodiment, as shown in FIG. Figure 3 As shown, before the fiber web is subjected to the pre-needling treatment, the main needling treatment and the cloth surface needling treatment in sequence to obtain the initial cloth, the method further includes:

[0057] Step S101: different types of fibers are fed into different bag opening machines according to production formulas, and the proportion of the input materials is controlled.

[0058] Optionally, different fibers (such as cotton, polyester, nylon, etc.) are mixed in precise proportions to achieve specific performance requirements, such as strength, moisture absorption, softness, etc. For example, adding a certain proportion of polyester fibers can improve the wear resistance and elasticity of the fabric, while cotton fibers can enhance comfort and moisture absorption and breathability. By controlling the proportions through the bale opener, the raw materials can be accurately delivered to ensure the consistency of subsequent product quality.

[0059] Step S102: metal detection is performed on different types of fibers that have passed through the bag opener, and the raw materials after detection are initially mixed and loosened through a mixing bin.

[0060] Optionally, metal detection is an important part of ensuring safe production, which can prevent metal foreign matter from mixing into the production process, damaging equipment or affecting product quality. Once metal impurities are detected, measures are taken immediately to remove them to ensure the purity of the fibers. Subsequently, through the mixing and opening process in the mixing bin, different fibers are fully contacted and mixed evenly, and fiber clumps are opened at the same time, improving the uniformity and efficiency of subsequent processing.

[0061] Step S103, further mixing and finely opening the fibers after mixing in the large bin.

[0062] Optionally, the mixing uniformity and opening degree of the fibers are further enhanced to ensure sufficient interweaving between the fibers, improve the fluffiness of the fiber layer and the uniformity of the subsequent web formation. This step helps to improve the uniformity and overall strength of the nonwoven fabric, and also provides a good fiber state for the subsequent molding process.

[0063] Step S104, the mixed and opened fibers are sucked into a cotton storage box through a fan for storage and standby use.

[0064] Optionally, the negative pressure of the fan can be used to transport the fibers to a cotton storage box, which reduces the labor intensity of manual handling and improves production efficiency. The cotton storage box serves as a temporary storage, which is convenient for timely supply of fiber raw materials according to production needs and ensures the continuity of the production process. At the same time, the cotton storage box can also isolate external pollution to a certain extent and keep the fibers clean.

[0065] Step S105: Send the fibers in the cotton storage box to the air pressure cotton box through a powerful fan, and accurately weigh the fibers through a belt scale.

[0066] Optionally, two powerful fans are used to deliver the fibers from the cotton storage box to the pneumatic cotton box, and the fibers are accurately weighed by a belt scale to ensure the uniformity of the product weight across the entire width. Specifically, the powerful fans ensure the continuity and speed of fiber transmission, and the pneumatic cotton box uses air flow pressure to maintain the loose state of the fibers, creating good conditions for the next processing (such as combing and web forming). The use of a belt scale enables accurate measurement of fiber weight, which is essential for controlling the weight and cost of finished products and ensuring the accuracy of the formula. Accurate weighing helps standardize production, reduce raw material waste, and ensure the stability of product quality.

[0067] Step S101 to step S105 constitute a fiber pretreatment process, which not only ensures product quality, but also improves production efficiency and economic benefits, laying a solid foundation for subsequent non-woven fabric manufacturing.

[0068] In one embodiment, in step S105, after the fibers in the cotton storage box are sent to the air pressure cotton box by a powerful fan and the fibers are accurately weighed by a belt scale, the method further comprises:

[0069] Step S106: The weighed different fibers are combed by a combing machine into a cross-arranged and evenly mixed single-layer fiber web.

[0070] Optionally, the carding machine combs, mixes and crosses the delivered fibers through the coordinated movement of a series of carding elements (such as carding rollers, fixed needle plates and movable needle plates). This process can effectively open the fiber bundles, remove impurities and lumps in the fibers, and make the fibers looser and more uniform. The fibers are transferred and combed multiple times during the carding process, achieving full mixing between the fibers and cross-arrangement of the fibers, which is conducive to improving the uniformity of subsequent web formation and the bonding force between the fibers. The staggered arrangement of the fibers increases the physical connection points, which improves the stability and strength of the fiber web.

[0071] In one embodiment, in step S106, the weighed different fibers are combed into a cross-arranged and evenly mixed single-layer fiber web by a combing machine, including:

[0072] Step S107: The single-layer fiber web is laid out into a multi-layer fiber web with a preset number of layers and uniform thickness by a web laying machine, and the multi-layer fiber web is overlapped.

[0073] Optionally, the web laying machine can precisely control the delivery and distribution of fibers to stack single-layer webs according to the preset number of layers and thickness requirements. Overlapping refers to the appropriate overlapping of the edges of multi-layer webs to ensure that the layers of fibers can be firmly combined together in subsequent processing (such as needle punching, hot melting, etc.) to prevent delamination or misalignment.

[0074] In one embodiment, in step S107, the weighed different fibers are combed by a combing machine into a cross-arranged and evenly mixed single-layer fiber web, including:

[0075] Step S108: using a drafting machine to change the arrangement of the fibers and arrange the fiber web in different ways.

[0076] Optionally, the drafting machine changes the arrangement and density distribution of the fibers in the web by stretching. This process can be uniaxial stretching or biaxial balanced or unbalanced stretching, depending on the performance requirements of the desired product. During the stretching process, the interaction forces between the fibers are readjusted, and the fibers may be further straightened, oriented or redistributed, thereby affecting the physical and mechanical properties of the web. The dimensional stability, strength and elongation of the web are improved, and by directional arrangement of the fibers, the strength and air permeability of the product can be optimized.

[0077] In one embodiment, step S109, the fiber web is subjected to a pre-needling treatment, a main-needling treatment and a cloth surface needle-punching treatment in sequence to obtain an initial cloth, wherein the pre-needling treatment and the main-needling treatment are used to adjust the fiber web structure, and the cloth surface needle-punching treatment is used to adjust the surface density and thickness of the fiber web. Specifically, it includes:

[0078] The pre-needling treatment has a needle puncture depth of 3.0-12.5 mm and a needle puncture density of 40-70 l / ㎡;

[0079] The puncture depth of the main puncture treatment is 2.5-8.0 mm, and the puncture density of the main puncture treatment is 120-200 l / ㎡;

[0080] The needle punching depth of the cloth surface needle punching treatment is 2.0-7.0 mm, and the needle punching density of the cloth surface needle punching treatment is 140-190 l / ㎡.

[0081] Optionally, the needling depth of the pre-needling treatment is set at 3.0-3.5 mm, and in this example, 3.5 mm can be selected. A deeper needling depth is helpful for the initial integration of fibers and the formation of a preliminary fiber interwoven structure.

[0082] After the initial formation of the fiber web, the pre-needling treatment uses a deep needling depth (3.0-12.5mm) and a lower needling density (40-70 l / ㎡), preferably a needling depth of 6-10mm and a density of 50-60 l / ㎡, to initially fix the fibers in the fiber web and establish basic fiber-to-fiber connections. The needling at this stage is intended to initially adjust the fiber web structure so that it has a certain degree of stability and processability. The main needling treatment uses a needling depth (2.5-8.0mm) and a higher needling density (120-200 l / ㎡), preferably a needling depth of 4-6mm and a density of 140-170 l / ㎡, in order to further strengthen the degree of interweaving of the fibers inside the fiber web and enhance the overall strength and structural stability of the fiber web. Needling with a higher density can form a denser structure. The needle punching depth (2.0-7.0mm) and density (140-190 l / ㎡) of the cloth surface needle punching treatment are preferably 3-5mm and 160-160 l / ㎡, mainly concentrated on the surface area of ​​the fiber web, in order to optimize the density and thickness of the fiber web surface and improve the appearance and feel of the product. This treatment adjusts the distribution of the surface fibers through slight surface needle punching, making the cloth surface smoother and denser.

[0083] Step S109 not only strengthens the fiber web from the internal structure, improves its physical performance indicators such as strength, thickness, weight and elongation, but also meets the high-quality requirements in surface treatment, ensuring that the fabric meets both functional and aesthetic standards, and provides high-quality raw materials for subsequent use or further processing. This step-by-step processing method reflects the strict control of details and quality in the nonwoven fabric production process.

[0084] In one embodiment, step S110, the initial fabric is dried by heating with circulating air in a closed space and controlling the oven temperature of the upper area and the lower area of ​​the fabric, and the drying is used to adjust the hardness of the fabric. Specifically, it includes:

[0085] Gas is used for heating in a closed space, and the oven temperatures of the upper area and the lower area of ​​the cloth are controlled separately by circulating air, wherein the oven temperatures of the upper area and the lower area of ​​the cloth are controlled according to the characteristics of the cloth, the oven temperature of the upper area of ​​the cloth includes 0°C-220°C, and the oven temperature of the lower area of ​​the cloth includes 0°C-220°C.

[0086] Optionally, gas is used as a heat source to heat the air in the enclosed space, and the hot air is circulated in the space by a circulating fan. This design ensures uniform heat distribution, avoids local overheating, and improves the utilization efficiency of thermal energy. According to the characteristics of the fabric, the oven temperature of the upper and lower areas of the fabric is independently controlled, and the range is set to 0°C to 220°C. The oven temperature of the upper area of ​​the fabric is preferably 180°C to 190°C, and the oven temperature of the lower area of ​​the fabric is preferably 140°C to 150°C. The oven temperature of the upper area of ​​the fabric is higher than that of the lower area of ​​the fabric. The temperature adjustment mechanism is based on the understanding of the water evaporation rate, fiber structure changes, and softness and hardness requirements during the drying process of the fabric. The upper temperature is often set higher to accelerate water evaporation and promote fiber redirection, thereby enhancing the hardness of the fabric; the lower temperature is relatively low, which helps to maintain the softness and structural stability of the fabric and prevent damage caused by overheating at the bottom. With the action of the circulating hot air, the moisture in the fabric is gradually evaporated, and the fibers undergo physical and chemical changes while losing moisture, which promotes the fixation of the structure and the adjustment of softness and hardness. The differential application of temperature speeds up the process and makes the final properties of the fabric more controllable.

[0087] Step S110 can precisely control the hardness of the fabric after drying by setting the difference in temperature between the upper and lower surfaces to meet the needs of different application scenarios. High temperature promotes tighter bonding between fibers and increases hardness, while low temperature helps retain the natural softness of the fabric. This not only optimizes the drying effect of the fabric and ensures that the hardness of the product meets specific needs, but also improves production efficiency and energy efficiency.

[0088] In one embodiment, step S111, surface treatment is performed on the dried fabric by a hot rolling roller, and the surface treatment is used to adjust the flatness of the fabric surface. Specifically, it includes:

[0089] Electric energy is used to circulate and heat the oil in the two hot rolling rollers, and the temperatures of the two hot rolling rollers are controlled respectively, and the upper and lower surfaces of the cloth are subjected to rolling treatment, wherein the temperature of the upper rolling roller in the hot rolling rollers includes 0℃-300℃, the temperature of the lower rolling roller in the hot rolling rollers includes 0℃-300℃, and the speed of the hot rolling rollers includes 3m / min-10m / min.

[0090] Optionally, the oil inside the hot roller is heated and circulated by electrical energy. This indirect heating method ensures that the heat energy is evenly distributed on the roller surface to avoid local overheating or uneven cooling. The oil circulation also plays a good role in heat conduction and heat preservation, so that the temperature of the hot roller can be accurately controlled. The upper and lower hot rollers are set to different temperature ranges (upper roller 190℃-200℃, lower roller 150℃-160℃). This temperature difference design can perform different degrees of heat treatment on the upper and lower surfaces of the cloth according to the characteristics of the cloth and the processing requirements. Higher temperatures help the plastic deformation and rearrangement of the fibers, while lower temperatures help maintain the stability of the cloth structure and avoid excessive heat treatment. The speed range of the hot roller is set at 3m / min-10m / min, and the speed is selected according to the thickness, material and desired surface effect of the cloth. Faster speeds are suitable for thinner fabrics or fabrics that require light smoothing to reduce fiber damage, while slower speeds are suitable for fabrics that require deep smoothing or thicker textures to ensure sufficient heat transfer and surface smoothness.

[0091] The hot roller surface treatment in step S111 achieves efficient flattening of the surface of the dried fabric through precise temperature and speed control, which not only improves the appearance quality of the fabric, but also optimizes its internal structure and functionality, effectively eliminates the unevenness and fine wrinkles on the fabric surface, and improves the smoothness and aesthetics of the fabric. Rollers with different temperatures act on the upper and lower surfaces of the fabric respectively, and can perform precise flattening according to the needs of different parts.

[0092] In one embodiment, before step S113, performing product quality inspection on the surface treated fabric, the method further comprises:

[0093] Step S112: evenly sprinkle powder on the surface of the fabric by a powder sprinkler.

[0094] Optionally, a powder spreader spreads powder (such as starch, rubber powder or other chemicals) evenly on the surface of the fabric by mechanical or pneumatic means. This equipment usually has a precise metering and distribution control system to ensure uniform coverage of the powder and avoid local excess or deficiency. One of the main purposes of powder spreading is to improve the surface properties of the fabric. For example, adding adhesive powders such as starch can enhance the adhesion between fibers, improve the stability of the fabric surface, and reduce hair loss or fiber shedding; while some functional powders can give fabrics waterproof, antistatic, antibacterial and other functions.

[0095] Step S112, sprinkling powder can improve the surface smoothness and feel of the fabric, and increase the aesthetics and tactile comfort of the product.

[0096] In one embodiment, step S113, product quality inspection is performed on the surface treated fabric, and fabric that does not meet the product quality standard is adjusted to obtain fabric that meets the product quality standard, wherein the product quality inspection includes fabric thickness, strength and elongation, gram weight, fabric hardness, fabric surface flatness and metal residue rate inspection. Specifically including:

[0097] When the thickness, shrinkage rate and gram weight of the fabric do not meet the quality standards, the needling depth and needling speed of the pre-needling treatment, the main needling treatment and the fabric surface needling treatment are adjusted;

[0098] When the hardness of the fabric does not meet the quality standard, adjusting the oven temperature of the upper area and the lower area of ​​the fabric;

[0099] When the surface flatness of the cloth does not meet the quality standard, adjusting the parameters of the surface treatment of the hot rolling roller;

[0100] In the case that the metal residue rate of the cloth does not meet the quality standard, the metal in the cloth is filtered and metal residue detection is performed on each device.

[0101] Optionally, the parameters of the needling treatment (pre-needling, main needling, and cloth surface needling) can be adjusted by analyzing whether the thickness, strength, elongation, and gram weight of the fabric meet the standards. Adjusting the needling depth and needling density can affect the interweaving density and structural compactness of the fibers, thereby indirectly controlling the thickness, gram weight, and stability of the fabric, and changing the strength and elongation. According to the test results of the softness and hardness of the fabric, the oven temperature of the upper and lower areas of the fabric is adjusted during the drying process, and the fine-tuning effect of temperature on the fiber structure is used to change the bonding force between the fibers and the physical state of the fibers, thereby achieving the purpose of adjusting the softness and hardness of the fabric. If the surface flatness does not meet the standards, the parameters of the hot roller treatment, including the temperature, pressure, and speed of the hot roller, need to be adjusted to optimize the distribution of the fibers on the surface, reduce wrinkles and unevenness, and improve the smoothness and uniformity of the fabric surface. For fabrics with excessive metal residues, filtering measures are taken to remove the mixed metal impurities, and metal detection and cleaning are performed on the equipment in the entire production process to prevent the reintroduction of metal impurities in future production and ensure product safety. In addition, when the powdering weight is uneven or the weight does not meet the preset weight, the powdering machine weight and speed parameters are adjusted, and the fiber arrangement can be adjusted through the drafting parameters of the drafting machine; the number of single-layer fiber laying layers can be adjusted through the number of laying machine layers; the product weight can be adjusted through the carding machine laying weight parameters.

[0102] Step S113 not only solves the quality problem of the current batch of products through precise testing and targeted adjustment strategies, but also accumulates valuable experience for subsequent production, ensuring the high quality and market competitiveness of nonwoven products. The cycle of testing and adjustment ensures that every step from raw materials to finished products can be strictly monitored and optimized, forming a closed-loop system of quality control and improving the qualification rate and consistency of the final product.

[0103] In one embodiment, after step S113, the method further includes:

[0104] Step S114 is to cut the product into products of specified width by a slitting machine, and remove the excess waste edges on both sides.

[0105] Optionally, the slitting machine uses a sharp blade or laser cutting technology to accurately cut continuous large-area nonwovens into strips or blocks according to pre-set width dimensions. This process requires high-precision positioning control and stable cutting speed to ensure that the cut edges are flat, burr-free, and accurate in size. Cutting off the excess waste edges on both sides is to remove possible defects or uneven parts on the edges of the fabric, which may not meet the quality requirements due to edge effects in the previous production process. After cutting, the overall quality of the product can be improved.

[0106] Step S115: The product is wound into a whole roll by a winding machine, and the quality department inspects and ships it after it passes the inspection.

[0107] Optionally, the winder mechanically winds the slit nonwoven strips or block products tightly and evenly into rolls. This process involves speed control, tension control and monitoring of winding diameter to ensure the compactness, flatness and uniformity of the roll. Before winding, there is usually a quality inspection link (including but not limited to defect detection and rejection equipment to remove defects in the product and effectively control defects and stains) to ensure that only qualified products enter the winding process and unqualified products will be rejected.

[0108] Step S114 and step S115 not only complete the transformation of the product from a large area to a specified size, but also ensure the high quality and standardization of the product through strict size control and quality inspection, laying a solid foundation for subsequent sales and use.

[0109] The following are specific practical application examples of the embodiments of this application:

[0110] Example 1: In order to develop a 100gsm-300gsm filter product required by customers, the front and back sides are required to be different in hardness and softness, and have different hand feel. In order to develop this product, this production line can be used to reasonably set the upper and lower temperatures of the oven and the upper and lower roller temperatures of the hot rolling mill to achieve this goal. The specific settings are: the upper zone temperature of the oven is 170℃-220℃, the lower zone temperature is 80℃-130℃, the upper roller temperature of the hot rolling mill is 170℃-220℃, the lower roller temperature is 80℃-130℃, and the speed is controlled at 6-7m / min, which can be appropriately reduced to 5-6m / min.

[0111] Example 2: In order to develop a 200gsm filter product required by customers, the front and back sides are required to be different in hardness and softness, and have different hand feel. In order to develop this product, this production line can be used to reasonably set the upper and lower temperatures of the oven and the upper and lower roller temperatures of the hot rolling mill to achieve this goal. The specific settings are: oven temperature upper zone 195℃, lower zone temperature 105℃, hot rolling mill temperature upper roller 195℃, lower roller 105℃, speed control at 6-7m / min, which can be appropriately reduced to 5-6m / min.

[0112] Example 3: In order to develop a product that the customer requires 300gsm-450gsm, one side is soft, the other side is hard, and it is not linted. To develop this product, this production line can be used to reasonably set the upper and lower temperatures of the oven and the upper and lower roller temperatures of the hot rolling mill to achieve this goal. The specific settings are: the upper zone temperature of the oven is 180℃-220℃, the lower zone temperature is 145℃-165℃, the upper roller temperature of the hot rolling mill is 180℃-220℃, the lower roller temperature is 145℃-165℃, and the speed is controlled at 3m / min-4m / min, and can be appropriately reduced.

[0113] Example 4: In order to develop a product that the customer requires 375gsm, one side is soft, the other side is hard, and it is not linted. To develop this product, this production line can be used to reasonably set the upper and lower temperatures of the oven and the upper and lower roller temperatures of the hot rolling mill to achieve this goal. The specific settings are: the upper zone temperature of the oven is 200℃, the lower zone temperature is 155℃, the upper roller temperature of the hot rolling mill is 200℃, the lower roller temperature is 155℃, and the speed is controlled at 3m / min-4m / min, and can be appropriately reduced.

[0114] In summary, the embodiment of the present application provides a method for controlling the quality of a needle-punched nonwoven fabric, wherein the fiber web is subjected to a pre-punching treatment, a main-punching treatment and a cloth surface needle-punching treatment in sequence to obtain an initial fabric, wherein the pre-punching treatment and the main-punching treatment are used to adjust the fiber web structure, and the cloth surface needle-punching treatment is used to adjust the surface density and thickness of the fiber web; the initial fabric is dried by circulating air heating in a confined space, and the oven temperature of the upper area and the lower area of ​​the fabric is controlled, and the drying is used to adjust the softness and hardness of the fabric; the dried fabric is surface-treated by a hot rolling roller, and the surface treatment is used to adjust the surface flatness of the fabric; the surface-treated fabric is subjected to product quality inspection, and fabrics that do not meet the product quality standards are adjusted accordingly to obtain fabrics that meet the product quality standards, wherein the product quality inspection includes fabric thickness, strength and elongation, gram weight, fabric softness and hardness, fabric surface flatness and metal residue rate inspection, so as to realize the control of the quality of the existing needle-punched nonwoven fabrics, effectively improve the quality of the nonwoven fabrics, and solve the problem of low quality of the existing needle-punched nonwoven fabrics in the related art.

[0115] The beneficial effects of the present invention also include: when unpacking, the proportion of raw materials is accurately controlled by a computer weighing system to ensure the accuracy of the formula. Before the materials enter the warehouse, a metal detector is used to detect whether there is metal in the materials to ensure the safety of the materials; when mixing in the warehouse, the materials are fully mixed by circulating air through a special fan to ensure the uniformity of the weight of the materials; before the air pressure cotton box enters the carding machine, it is accurately weighed by a belt scale to ensure uniform weight; before winding, metal and defect detection and removal equipment are added to remove defects in the product to effectively control defects and stains. Under the effective control of this process, the product can meet the expected quality standards, greatly reduce downstream product production losses and consumer complaints, the product weight is stable, the strength and elongation indicators meet the standards, and defects, metals and stains can be effectively removed.

[0116] This approach can bring the following practical benefits:

[0117] 1. Reducing the scrap rate of needle-punched non-woven fabrics can effectively reduce the scrap rate to below 6%, indirectly reducing production costs and labor costs for enterprises, saving production time and improving production efficiency.

[0118] Second, price increase due to stable quality. Due to stable quality, products can be sold to high-end companies that are not sensitive to prices, opening up the application market and increasing corporate profits.

[0119] 3. Indirectly improve the competitiveness of enterprises. Stable quality can reduce customer and consumer complaints, improve corporate image and competitiveness, and provide financial guarantees for the long-term development of enterprises.

[0120] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0121] The above embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.

Claims

1. A method for controlling the quality of needle-punched nonwoven fabrics, characterized in that: The method comprises: The fiber web is sequentially subjected to a pre-needling treatment, a main-needling treatment and a cloth surface needle-punching treatment to obtain an initial fabric, wherein the pre-needling treatment and the main-needling treatment are used to adjust the fiber web structure, and the cloth surface needle-punching treatment is used to adjust the surface density and thickness of the fiber web; The initial fabric is dried by heating with circulating air in a closed space and controlling the oven temperature of the upper area and the lower area of ​​the fabric, wherein the drying is used to adjust the hardness of the fabric; The dried fabric is subjected to surface treatment by means of a hot roller, wherein the surface treatment is used to adjust the flatness of the fabric surface; Perform product quality inspection on the surface-treated fabrics, make relevant adjustments to the fabrics that do not meet the product quality standards, and obtain fabrics that meet the product quality standards, wherein the product quality inspection includes fabric thickness, strength and elongation, gram weight, fabric hardness, fabric surface flatness and metal residue rate inspection; Among them, making relevant adjustments to the fabric that does not meet the product quality standards to obtain the fabric that meets the product quality standards, including: when the thickness, strength, elongation and gram weight of the fabric do not meet the quality standards, adjusting the needle depth and needle density of the pre-needling treatment, the main needle treatment and the fabric surface needle treatment; when the hardness of the fabric does not meet the quality standards, adjusting the oven temperature of the upper area and the lower area of ​​the fabric; when the surface flatness of the fabric does not meet the quality standards, adjusting the parameters of the hot rolling roller surface treatment; when the metal residue rate of the fabric does not meet the quality standards, filtering the metal in the fabric and performing metal residue detection on each device; The needle depth of the pre-needling treatment is 3.0-12.5mm, and the needle density of the pre-needling treatment is 40-70 l / ㎡; the needle depth of the main needle treatment is 2.5-8.0mm, and the needle density of the main needle treatment is 120-200 l / ㎡; the needle depth of the cloth surface needle treatment is 2.0-7.0mm, and the needle density of the cloth surface needle treatment is 140-190 l / ㎡; The method of drying the initial fabric by heating with circulating air in a closed space and controlling the oven temperatures of the upper and lower regions of the fabric comprises: heating with gas in a closed space and controlling the oven temperatures of the upper and lower regions of the fabric respectively by circulating air, wherein the oven temperatures of the upper and lower regions of the fabric are controlled according to the fabric characteristics, the oven temperature of the upper region of the fabric being within a range of 0°C to 220°C, and the oven temperature of the lower region of the fabric being within a range of 0°C to 220°C; The dried fabric is surface treated by hot rolling rollers, and the surface treatment is used to adjust the surface flatness of the fabric, including: using electric energy to circulate and heat the oil in two hot rolling rollers, respectively controlling the temperatures of the two hot rolling rollers, and performing rolling treatment on the upper and lower surfaces of the fabric, wherein the temperature of the upper rolling roller in the hot rolling rollers includes 0°C-300°C, the temperature of the lower rolling roller in the hot rolling rollers includes 0°C-300°C, and the speed of the hot rolling rollers includes 3m / min-10m / min.

2. The method according to claim 1, characterized in that: Before performing product quality inspection on the surface-treated fabric, the method further comprises: The surface of the cloth is evenly powdered by a powder spreading machine.

3. The method according to claim 1, characterized in that Before the fiber web is subjected to the pre-needling treatment, the main needling treatment and the cloth surface needling treatment in sequence to obtain the initial cloth, the method further comprises: Different types of fibers are fed into different bale opening machines according to the production formula, and the proportion of input materials is controlled; The different types of fibers that pass through the bale opener are subjected to metal detection, and the raw materials after detection are initially mixed and loosened through the mixing bin; Further mixing and finely opening the fibers after mixing in the large bin; The mixed and opened fibers are sucked into a cotton storage box through a fan for storage and standby; The fibers in the cotton storage box are sent to the air pressure cotton box by a powerful fan, and the fibers are accurately weighed by a belt scale.

4. The method according to claim 3, characterized in that After the fibers in the cotton storage box are sent to the air pressure cotton box by a powerful fan and the fibers are accurately weighed by a belt scale, the method further comprises: The weighed different fibers are combed into a cross-arranged, evenly mixed single-layer fiber web through a carding machine.

5. The method according to claim 4, characterized in that The weighed different fibers are combed into a cross-arranged, evenly mixed single-layer web through a carding machine, including: A single-layer fiber web is laid out by a web laying machine into a multi-layer fiber web with a preset number of layers and uniform thickness, and the multi-layer fiber web is overlapped.

6. The method according to claim 5, characterized in that After the single-layer fiber web is laid by a web laying machine into a multi-layer fiber web with a preset number of layers and uniform thickness, and the multi-layer fiber web is overlapped, the method further comprises: The fiber web is arranged differently by changing the arrangement of the fibers through a drafting machine.

Citation Information

Patent Citations

  • Manufacturing method of non-woven needling adhesive tape substrate

    CN103451854A

  • Multipurpose functional nonwoven fiber, and method for manufacturing same

    CN103827374A

  • Preparation method of needle punched non-woven fabric

    CN105401334A

  • Production method of water-repellent oil-proof needled felt filter material

    CN107557997A

  • Preparation method of non-woven fabric

    CN108035068A