A guide with a hollow blade structure and a method for producing the same

By separately pressing the ceramic core and the turbine guide wax mold, the problems of complex wax molds and core breakage due to eccentricity in the existing technology are solved, realizing the efficient and low-cost preparation of hollow blade turbine guides, which is suitable for the field of precision casting.

CN118543791BActive Publication Date: 2026-11-24AVIC BEIJING INST OF AERONAUTICAL MATERIALS
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410806284.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2026-11-24
Estimated Expiration
2044-06-21

AI Technical Summary

Technical Problem

Existing technologies for manufacturing hollow blade turbine guide vanes involve complex wax mold structures, long pressing cycles, and are prone to problems such as core misalignment and core breakage. Furthermore, additional X-ray inspection is required, resulting in low efficiency and high costs.

Method used

The method of separately pressing ceramic cores and turbine guide wax molds is adopted. The ceramic cores are inserted into the hollow blade cavity of the wax mold, and the gating system is connected by welding to prepare the mold shell as a whole and then pouring. This avoids core deviation and core breakage and simplifies the design of wax molds.

Benefits of technology

It improves manufacturing efficiency, reduces costs, ensures the consistency of hollow structures, avoids X-ray inspection, and is suitable for hollow structure parts in the field of precision casting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118543791B_ABST
    Figure CN118543791B_ABST
Patent Text Reader

Abstract

This invention discloses a guide with a hollow blade structure and its manufacturing method. The guide includes an integrally formed lower flow channel, upper flow channel, exhaust flange, and hollow blades, with a plurality of hollow blades evenly distributed along the axial direction between the lower and upper flow channels. The manufacturing method includes the following steps: pressing a plurality of ceramic cores and a hollow blade turbine guide wax model; inserting the plurality of ceramic cores into the hollow blades on the hollow blade turbine guide wax model, with the entire molded portion inserted into the hollow blade cavity, the limiting step matching the opening end of the hollow blade cavity, and the free end portion exposed outside the hollow blade cavity; repairing the gap between the limiting step and the lower flow channel; assembling the gating system onto the exhaust flange end face; preparing the mold shell, melting and casting, and chemically removing the cores to obtain the guide with the hollow blade structure. This invention avoids the problems of core misalignment and core breakage that occur during wax pressing, wax filling, and casting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of guide preparation technology, specifically relating to a guide with a hollow blade structure and its preparation method. Background Technology

[0002] As is well known, turbine guide vanes are one of the most critical hot-end components in aero-engines and gas turbines. To meet the ever-increasing power-to-weight ratio requirements of engines, these hot-end components need to be developed towards integration and lightweight design. Simultaneously, the continuous increase in turbine inlet temperature is also driving the development of guide vane blades from solid to hollow structures. Currently, hollow turbine guide vanes are typically manufactured using investment casting.

[0003] The existing process for manufacturing hollow blade turbine guides is as follows: first, a core is prepared; then, the core and a wax model are pressed together; after pressing, the wax model is inspected using X-rays; then, the wax model is corrected and combined; finally, the shell is prepared and the melting and casting processes are carried out. The existing technology is suitable for manufacturing guides with relatively complex hollow cavity structures. However, for the guide of this invention, the existing technology has the following drawbacks: (1) the required wax model mold has a complex structure; (2) the pressing cycle for a single wax model is long and inefficient; (3) during the pressing process, the core is prone to deviating or breaking; (4) the pressed wax model needs to be inspected for core breakage, increasing the manufacturing cycle and cost. Therefore, it is necessary to develop a guide with a hollow blade structure and its manufacturing method to solve the problems existing in the existing technology.

[0004] Chinese patent application CN107989661A discloses a guide, comprising an inner ring, an outer ring, and multiple hollow blades located between the outer edge of the inner ring and the inner edge of the outer ring. The hollow blades extend radially along the guide. Each hollow blade includes an upper edge, an upper surface, a lower surface, and a lower edge. The upper edge extends radially along the guide and protrudes counterclockwise, as does the lower edge. The upper ends of the upper and lower surfaces converge at the upper edge, and the lower ends of the upper and lower surfaces converge at the lower edge. The lower surface has bolt holes, and the inner wall of the upper surface has bolt connecting seats corresponding to the bolt holes. The bolt holes and bolt connecting seats are connected by bolts, and a spring is sleeved on the bolt, with the spring located between the bolt holes and the bolt connecting seats. This guide is an axial flow guide, with a relatively complex internal structure, making it impossible to directly insert a core. Furthermore, each hollow blade is composed of two parts and cannot be cast as a single piece. Summary of the Invention

[0005] To address the problems existing in the prior art, the present invention provides a guide with a hollow blade structure, comprising an integrally formed lower flow channel, an upper flow channel, an exhaust flange, and hollow blades; the lower flow channel is a flat plate structure with a through hole in the center, the upper flow channel is a disc structure with a through hole in the center, and the exhaust flange is a cylindrical structure; the central axis of the lower flow channel, the central axis of the upper flow channel, and the central axis of the exhaust flange are located on the same straight line; a plurality of hollow blades are evenly distributed along the axial direction between the lower flow channel and the upper flow channel.

[0006] Preferably, the interior of the hollow blade is a hollow blade cavity, which is a blind hole structure with its open end located on the lower flow channel; a ceramic core is inserted into the hollow blade cavity from its open end.

[0007] In any of the above embodiments, it is preferred that the ceramic core includes an integrally formed profile portion, a limiting step, and a free end portion, wherein the limiting step is located between the profile portion and the free end portion.

[0008] In any of the above embodiments, it is preferred that the profiled portion matches the cavity of the hollow blade, the limiting step matches the opening end of the cavity of the hollow blade, and hand-held grooves are respectively provided on both sides of the free end portion.

[0009] In any of the above embodiments, it is preferred that the vent flange is connected to the gating system.

[0010] The present invention also provides a method for preparing a guide with a hollow blade structure, for preparing the guide with a hollow blade structure as described in any of the above claims, comprising the following steps in sequence:

[0011] Step 1: Design a ceramic core mold according to the requirements, and then use the ceramic core mold to press several ceramic cores;

[0012] Step 2: Design the hollow blade turbine guide wax mold according to the requirements, and then use the hollow blade turbine guide wax mold to press the hollow blade turbine guide wax model.

[0013] Step 3: Insert several ceramic cores into several hollow blades on the hollow blade turbine guide wax model. The entire surface of the ceramic core is inserted into the cavity of the hollow blade, and the surface matches the cavity. The limiting step of the ceramic core matches the opening end of the cavity. The free end of the ceramic core is exposed outside the cavity.

[0014] Step 4: After all the ceramic cores have been inserted into the hollow blades on the hollow blade turbine guide wax mold, use glue or wax to repair the gap between the limiting step and the lower flow channel so that the molded part is fixed in the hollow blade cavity.

[0015] Step 5: Assemble the casting system onto the exhaust end flange face of the hollow blade turbine guide vane wax model by welding;

[0016] Step Six: Prepare a mold shell on the outer surface of the hollow blade turbine guide wax model, ceramic core, and gating system as a whole;

[0017] Step 7: Wrap cotton on the outer side of the mold shell corresponding to the gating system, then put the mold shell into the preheating furnace for preheating treatment. After the preheating treatment is completed, transfer the mold shell to the casting furnace for casting.

[0018] Step 8: After the casting is completed, the casting is water-blown and shell-cleaned. At the same time, the gating system is cut off. Then, the casting is chemically cored and the residual core in the hollow blade cavity is removed to obtain a guide with a hollow blade structure.

[0019] Preferably, in step one, the pressing parameters of the ceramic core include a pressing temperature of 60-120℃, an injection pressure of 1-10MPa, and a holding time of 10-60s; after the ceramic core is pressed, it needs to be sintered at a temperature of 500-1000℃ for 2-15h.

[0020] In any of the above schemes, it is preferred that, in step two, the pressing parameters of the hollow blade turbine guide wax mold include: wax pressing temperature of 50-80℃, wax injection pressure of 5-30 bar, and holding time of 30-120 s.

[0021] In any of the above schemes, the preferred method is that, in step six, the preparation process of the mold shell is as follows: the hollow blade turbine guide wax mold, ceramic core and casting system are treated as a whole, 5-9 layers of refractory slurry are applied to its outer surface, and after coating, it is naturally dried for 6-12 hours. After drying, it is dewaxed at a temperature of 100-200℃, and after dewaxing, it is calcined at a temperature of 900-1100℃ for 2-6 hours to obtain the mold shell. The inside of the mold shell is flushed or blown cleaned to remove foreign inclusions, and then naturally air-dried for 6-10 hours.

[0022] In any of the above schemes, it is preferred that, in step seven, the cotton wrapping thickness is 6-26mm; the preheating temperature is 900-1200℃, the heat preservation time is 2-5h; and the pouring temperature is 1400-1600℃.

[0023] The preheating furnace and casting furnace used in this invention are all commonly used equipment in the field, and no special requirements are made regarding their models. In the ceramic core, the molded surface portion is inserted into the hollow blade cavity of the wax model to form the hollow blade cavity structure during subsequent casting. The limiting step is used to limit the insertion depth of the molded surface portion, ensuring that the entire molded surface portion is inserted into the hollow blade cavity. The free end portion protrudes outside the wax model and plays a holding role during the insertion of the molded surface portion into the hollow blade cavity. It also plays a fixing role during the subsequent preparation of the mold shell, preventing the molded surface portion from shifting and causing core misalignment.

[0024] In step two, when designing the wax mold for the hollow blade turbine guide vane, a special movable block for forming the hollow blade cavity structure must be designed. This special movable block consists of a movable block for forming the hollow blade cavity and a movable block for forming part of the lower flow channel. Considering the subsequent insertion of the molded surface portion into the hollow blade cavity on the wax mold, a gap of 0.05-0.1mm needs to be reserved when designing the movable block for forming the hollow blade cavity to ensure that the molded surface portion can be inserted without damaging the wax mold. At the same time, to prevent the hollow blade cavity portion on the wax mold from being unable to be pulled out due to negative pressure during demolding, an venting insert needs to be set on the movable block for forming the hollow blade cavity, and venting grooves need to be made around the insert.

[0025] In step three, several ceramic cores are inserted into several hollow blades on the hollow blade turbine guide wax model. The entire surface of the ceramic core is inserted into the cavity of the hollow blade, and the surface matches the cavity. The limiting step of the ceramic core matches the opening end of the hollow blade cavity, while the free end of the ceramic core protrudes outside the cavity. Step three is a crucial step in the fabrication of the hollow blade turbine guide. The pressing and sintering parameters of the ceramic core, the pressing parameters of the hollow blade turbine guide wax model, the mold shell preparation parameters, and the casting parameters are also very important. Only by coordinating the various process steps and parameters can the intended technical effect of this invention be achieved.

[0026] The present invention relates to a guide with a hollow blade structure and a method for its preparation, which has the following beneficial effects:

[0027] (1) In this invention, the ceramic core and the turbine guide wax mold are pressed separately and independently, and then the ceramic core is inserted into the hollow blade cavity of the turbine guide wax mold. This method can avoid the problems of core deviation and core breakage during the wax pressing, wax filling and pouring process, and the overall processability is better; while the method of pressing the ceramic core and the wax mold as a whole is easy to produce core deviation and core breakage problems.

[0028] (2) The preparation method of the present invention does not require X-ray inspection of the wax model product, which shortens the manufacturing cycle and reduces the manufacturing cost; while the method of pressing the ceramic core and the wax model as a whole requires X-ray inspection of the wax model product.

[0029] (3) The mold for pressing ceramic cores in this invention is simple and the resulting hollow structure has good consistency.

[0030] (4) The preparation method of the present invention can be extended to hollow structure parts of the same type in the field of precision casting, such as straight hole structure, which can effectively reduce the manufacturing cost and manufacturing difficulty of this type of product. Attached Figure Description

[0031] Figure 1 This is a schematic diagram of a preferred embodiment of a guide with a hollow blade structure according to the present invention;

[0032] Figure 2 for Figure 1 A schematic diagram of the guide with a hollow blade structure in the illustrated embodiment from another perspective;

[0033] Figure 3 for Figure 1 A schematic diagram of the ceramic core in the illustrated embodiment;

[0034] Figure 4 for Figure 1 The illustrated embodiment shows a schematic diagram of inserting a ceramic core into a hollow blade on a hollow blade turbine guide wax model;

[0035] Figure 5 for Figure 1 A schematic diagram of the overall structure of the hollow blade turbine guide wax model, ceramic core, and gating system in the embodiment shown;

[0036] Figure 6 for Figure 1 A schematic diagram of a special movable block for forming the hollow blade cavity structure in the embodiment shown;

[0037] Figure 7 for Figure 1 A photograph of a turbine guide with a hollow blade structure prepared according to the embodiment shown.

[0038] Figure 8 for Figure 1 The photograph shows an inspection image of a turbine guide with a hollow blade structure prepared according to the embodiment shown.

[0039] Explanation of annotations in the image:

[0040] 1- Turbine guide vane with hollow blade structure, 101- Lower flow channel, 102- Upper flow channel, 103- Exhaust end flange, 104- Hollow blade, 105- Hollow blade cavity;

[0041] 2-Ceramic core, 201-Mold surface, 202-Limiting step, 203-Free end, 204-Handheld groove;

[0042] 3-Gating system;

[0043] 4-A special movable block for forming the hollow blade cavity structure; 401-A movable block for forming the hollow blade cavity; 402-A movable block for forming part of the lower flow channel. Detailed Implementation

[0044] To further understand the invention, the following detailed description of the invention will be provided in conjunction with specific embodiments.

[0045] Example 1:

[0046] like Figure 1-5 As shown, according to a preferred embodiment of the guide vane with a hollow blade structure of the present invention, the turbine guide vane 1 with a hollow blade structure includes an integrally formed lower flow channel 101, an upper flow channel 102, an exhaust end flange 103, and hollow blades 104; the lower flow channel 101 is a flat plate structure with a through hole in the center, the upper flow channel 102 is a disc structure with a through hole in the center, and the exhaust end flange 103 is a cylindrical structure. The central axis of the lower flow channel 101, the central axis of the upper flow channel 102, and the central axis of the exhaust end flange 103 are located on the same straight line; a plurality of hollow blades 104 are evenly distributed along the axial direction between the lower flow channel 101 and the upper flow channel 102. The exhaust end flange 103 is connected to the casting system 3.

[0047] The interior of the hollow blade 104 is a hollow blade cavity 105, which is a blind hole structure with its open end located on the lower flow channel 101; a ceramic core 2 is inserted into the hollow blade cavity 105 from its open end.

[0048] The ceramic core 2 includes an integrally formed profile portion 201, a limiting step 202, and a free end portion 203. The limiting step 202 is located between the profile portion 201 and the free end portion 203. The profile portion 201 matches the hollow blade cavity 105, and the limiting step 202 matches the open end of the hollow blade cavity 105. Handheld grooves 204 are respectively provided on both sides of the free end portion 203.

[0049] This embodiment also provides a method for preparing a guide with a hollow blade structure, which includes the following steps in sequence:

[0050] Step 1: Design a ceramic core mold according to the requirements, and then use the ceramic core mold to press several ceramic cores;

[0051] Step 2: Design the hollow blade turbine guide wax mold according to the requirements, and then use the hollow blade turbine guide wax mold to press the hollow blade turbine guide wax model.

[0052] Step 3: Insert several ceramic cores into several hollow blades on the hollow blade turbine guide wax model. The entire surface of the ceramic core is inserted into the cavity of the hollow blade, and the surface matches the cavity. The limiting step of the ceramic core matches the opening end of the cavity. The free end of the ceramic core is exposed outside the cavity.

[0053] Step 4: After all the ceramic cores have been inserted into the hollow blades on the hollow blade turbine guide wax mold, use glue or wax to repair the gap between the limiting step and the lower flow channel so that the molded part is fixed in the hollow blade cavity.

[0054] Step 5: Assemble the casting system onto the exhaust end flange face of the hollow blade turbine guide vane wax model by welding;

[0055] Step Six: Prepare a mold shell on the outer surface of the hollow blade turbine guide wax model, ceramic core, and gating system as a whole;

[0056] Step 7: Wrap cotton on the outer side of the mold shell corresponding to the gating system, then put the mold shell into the preheating furnace for preheating treatment. After the preheating treatment is completed, transfer the mold shell to the casting furnace for casting.

[0057] Step 8: After the casting is completed, the casting is water-blown and shell-cleaned. At the same time, the gating system is cut off. Then, the casting is chemically cored and the residual core in the hollow blade cavity is removed to obtain a guide with a hollow blade structure.

[0058] In step one, the pressing parameters of the ceramic core include a pressing temperature of 90°C, an injection pressure of 5MPa, and a holding time of 35s. After the ceramic core is pressed, it needs to be sintered at a temperature of 800°C for 8 hours.

[0059] In step two, the pressing parameters of the hollow blade turbine guide wax mold include: wax pressing temperature of 65°C, wax injection pressure of 20 bar, and holding time of 75 s.

[0060] In step six, the preparation process of the mold shell is as follows: the hollow blade turbine guide wax mold, ceramic core and casting system are treated as a whole, and 7 layers of refractory slurry are applied to its outer surface. After coating, it is naturally dried for 9 hours. After drying, it is dewaxed at 150°C. After dewaxing, it is fired at 1000°C for 4 hours to obtain the mold shell. The inside of the mold shell is flushed or blown cleaned to remove foreign inclusions, and then naturally air-dried for 8 hours.

[0061] In step seven, the cotton wrapping thickness is 16mm; the preheating temperature is 1050℃, the holding time is 3h; and the pouring temperature is 1500℃.

[0062] The preheating furnace and casting furnace used in this embodiment are all commonly used equipment in the field, and there are no special requirements for their models. In the ceramic core, the molded surface portion is inserted into the hollow blade cavity of the wax model to form the hollow blade cavity structure during subsequent casting. The limiting step is used to limit the insertion depth of the molded surface portion, ensuring that the entire molded surface portion is inserted into the hollow blade cavity. The free end portion protrudes outside the wax model and plays a holding role during the insertion of the molded surface portion into the hollow blade cavity. It also plays a fixing role during the subsequent preparation of the mold shell to prevent the molded surface portion from shifting and causing core misalignment.

[0063] In step two, when designing the wax mold for the hollow blade turbine guide vane, a special movable block 4 must be designed to form the hollow blade cavity structure. The specific structure is as follows: Figure 6 As shown, the special movable block consists of a movable block 401 that forms the hollow blade cavity and a movable block 402 that forms part of the lower flow channel. Considering the subsequent insertion of the molded surface portion into the hollow blade cavity on the wax model, a gap of 0.05-0.1mm needs to be reserved when designing the movable block that forms the hollow blade cavity to ensure that the molded surface portion can be inserted without damaging the wax model. At the same time, in order to prevent the hollow blade cavity portion on the wax model from being unable to be pulled out due to negative pressure during demolding, an venting insert needs to be set on the movable block that forms the hollow blade cavity, and venting grooves are made around the insert.

[0064] In step three, several ceramic cores are inserted into several hollow blades on the hollow blade turbine guide wax model. The entire surface of the ceramic core is inserted into the cavity of the hollow blade, and the surface matches the cavity. The limiting step of the ceramic core matches the opening end of the hollow blade cavity, while the free end of the ceramic core protrudes outside the cavity. Step three is a crucial step in the fabrication of the hollow blade turbine guide. The pressing and sintering parameters of the ceramic core, the pressing parameters of the hollow blade turbine guide wax model, the mold shell preparation parameters, and the casting parameters are also very important. Only by coordinating the various process steps and parameters can the expected technical effect of this embodiment be achieved.

[0065] A photograph of the guide with a hollow blade structure prepared in this embodiment is shown below. Figure 7 As shown, its detection photos are as follows Figure 8 As shown, from Figure 8 It can be seen that the wall thickness on both sides of the hollow blade cavity is consistent and uniform, and the hollow blade cavity is complete with no residual core inside. This indicates that the hollow blade turbine guide vane prepared by the preparation method of this embodiment will not produce problems such as core deviation or core breakage.

[0066] This embodiment of the guide with a hollow blade structure and its preparation method has the following beneficial effects: (1) The ceramic core and the turbine guide wax model are pressed separately and independently, and then the ceramic core is inserted into the hollow blade cavity of the turbine guide wax model, which can avoid the problems of core deviation and core breakage during wax pressing, wax filling, and casting, and the overall processability is better. (2) There is no need to perform X-ray inspection on the wax model product, which shortens the manufacturing cycle and reduces the manufacturing cost. (3) The mold used to press the ceramic core is simple, and the hollow structure formed has good consistency. (4) It can be extended to the field of precision casting for similar hollow structure parts, which can effectively reduce the manufacturing cost and manufacturing difficulty of this type of product.

[0067] Example 2:

[0068] According to another preferred embodiment of the guide with hollow blade structure and its preparation method of the present invention, the structure, preparation steps, technical principles, and beneficial effects of the prepared guide are basically the same as those of Embodiment 1, except that:

[0069] In step one, the pressing parameters of the ceramic core include a pressing temperature of 60°C, an injection pressure of 1 MPa, and a holding time of 60 seconds. After the ceramic core is pressed, it needs to be sintered at a temperature of 500°C for 15 hours.

[0070] In step two, the pressing parameters of the hollow blade turbine guide wax mold include: wax pressing temperature of 50°C, wax injection pressure of 5 bar, and holding time of 120 seconds.

[0071] In step six, the preparation process of the mold shell is as follows: the hollow blade turbine guide wax mold, ceramic core and casting system are treated as a whole, and five layers of refractory slurry are applied to its outer surface. After coating, it is naturally dried for 6 hours. After drying, it is dewaxed at 100°C. After dewaxing, it is fired at 900°C for 6 hours to obtain the mold shell. The inside of the mold shell is flushed or blown cleaned to remove foreign inclusions, and then naturally air-dried for 6 hours.

[0072] In step seven, the cotton wrapping thickness is 6mm; the preheating temperature is 900℃, the holding time is 5h; and the pouring temperature is 1400℃.

[0073] Example 3:

[0074] According to another preferred embodiment of the guide with hollow blade structure and its preparation method of the present invention, the structure, preparation steps, technical principles, and beneficial effects of the prepared guide are basically the same as those of Embodiment 1, except that:

[0075] In step one, the pressing parameters of the ceramic core include a pressing temperature of 120°C, an injection pressure of 10MPa, and a holding time of 10s. After the ceramic core is pressed, it needs to be sintered at a temperature of 1000°C for 2 hours.

[0076] In step two, the pressing parameters of the hollow blade turbine guide wax mold include: wax pressing temperature of 80℃, wax injection pressure of 30 bar, and holding time of 30 s.

[0077] In step six, the preparation process of the mold shell is as follows: the hollow blade turbine guide wax mold, ceramic core and casting system are treated as a whole, and nine layers of refractory slurry are applied to its outer surface. After coating, it is naturally dried for 12 hours. After drying, it is dewaxed at 200°C. After dewaxing, it is fired at 1100°C for 2 hours to obtain the mold shell. The inside of the mold shell is rinsed or blown cleaned to remove foreign inclusions, and then naturally air-dried for 10 hours.

[0078] In step seven, the cotton wrapping thickness is 26mm; the preheating temperature is 1200℃, the holding time is 2h; and the pouring temperature is 1600℃.

[0079] Special Note: The technical solution of this invention involves numerous parameters, and the synergistic effects between these parameters must be comprehensively considered to achieve the beneficial effects and significant progress of this invention. Furthermore, the value ranges of each parameter in the technical solution were obtained through extensive experimentation. For each parameter and the combinations thereof, the inventors have recorded a large amount of experimental data; however, due to space limitations, the specific experimental data is not disclosed here.

[0080] Those skilled in the art will readily understand that the guide with a hollow blade structure and its preparation method of the present invention include any combination of the inventive content and specific embodiments described in the above specification and the various parts shown in the accompanying drawings. Due to space limitations and for the sake of brevity, not all of these combinations have been described in detail. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.

Claims

1. A method for manufacturing a guide with a hollow blade structure, characterized in that, The preparation method includes the following steps in sequence: Step 1: Design a ceramic core mold according to the requirements, and then use the ceramic core mold to press several ceramic cores; Step 2: Design the hollow blade turbine guide wax mold according to the requirements, and then use the hollow blade turbine guide wax mold to press the hollow blade turbine guide wax model. Step 3: Insert several ceramic cores into several hollow blades on the hollow blade turbine guide wax model. The entire surface of the ceramic core is inserted into the cavity of the hollow blade, and the surface matches the cavity. The limiting step of the ceramic core matches the opening end of the cavity. The free end of the ceramic core is exposed outside the cavity. Step 4: After all the ceramic cores have been inserted into the hollow blades on the hollow blade turbine guide wax mold, use glue or wax to repair the gap between the limiting step and the lower flow channel so that the molded part is fixed in the hollow blade cavity. Step 5: Assemble the casting system onto the exhaust end flange face of the hollow blade turbine guide vane wax model by welding; Step Six: Prepare a mold shell on the outer surface of the hollow blade turbine guide wax model, ceramic core, and gating system as a whole; Step 7: Wrap cotton on the outer side of the mold shell corresponding to the gating system, then put the mold shell into the preheating furnace for preheating treatment. After the preheating treatment is completed, transfer the mold shell to the casting furnace for casting. Step 8: After the casting is completed, the casting is water-blown and shell-cleaned. At the same time, the gating system is cut off. Then, the casting is chemically cored and the residual core in the hollow blade cavity is removed to obtain a guide with a hollow blade structure. The guide with a hollow blade structure includes an integrally formed lower flow channel, upper flow channel, exhaust flange, and hollow blades; the lower flow channel is a flat plate structure with a through hole in the center, the upper flow channel is a disc structure with a through hole in the center, and the exhaust flange is a cylindrical structure. The central axis of the lower flow channel, the central axis of the upper flow channel, and the central axis of the exhaust flange are located on the same straight line; a plurality of hollow blades are evenly distributed along the axial direction between the lower flow channel and the upper flow channel. The interior of the hollow blade is a hollow blade cavity, which is a blind hole structure. Its open end is located on the lower flow channel, and a ceramic core is inserted into the hollow blade cavity from the open end. The ceramic core includes an integrally formed profile portion, a limiting step, and a free end portion, wherein the limiting step is located between the profile portion and the free end portion; The profiled portion matches the cavity of the hollow blade, the limiting step matches the opening end of the cavity of the hollow blade, and hand-held grooves are provided on both sides of the free end portion.

2. The method for preparing a guide with a hollow blade structure according to claim 1, characterized in that, In step one, the pressing parameters of the ceramic core include: pressing temperature of 60-120℃, injection pressure of 1-10MPa, and holding time of 10-60s; after the ceramic core is pressed, it needs to be sintered at a temperature of 500-1000℃ for 2-15h.

3. The method for preparing a guide with a hollow blade structure according to claim 2, characterized in that, In step two, the pressing parameters of the hollow blade turbine guide wax mold include: wax temperature of 50-80℃, wax injection pressure of 5-30 bar, and holding time of 30-120 s.

4. The method for preparing a guide with a hollow blade structure according to claim 3, characterized in that, In step six, the preparation process of the mold shell is as follows: the hollow blade turbine guide wax mold, ceramic core and casting system are treated as a whole, and 5-9 layers of refractory slurry are applied to its outer surface. After coating, it is naturally dried for 6-12 hours. After drying, it is dewaxed at a temperature of 100-200℃. After dewaxing, it is fired at a temperature of 900-1100℃ for 2-6 hours to obtain the mold shell. The inside of the mold shell is flushed or blown cleaned to remove foreign inclusions, and then naturally air-dried for 6-10 hours.

5. The method for preparing a guide with a hollow blade structure according to claim 4, characterized in that, In step seven, the cotton wrapping thickness is 6-26mm; the preheating temperature is 900-1200℃, the heat preservation time is 2-5h; and the pouring temperature is 1400-1600℃.

Citation Information

Patent Citations

  • Guider

    CN107989661A

  • Lost wax casting method for nozzle ring

    KR101358278B1

  • Turbomachines having guide ducts

    US20140234094A1