A liner for realizing precise forming of EFP by mechanical property gradient

By using a shaped charge liner with gradually varying mechanical properties, the problem of necking and fracture during EFP detonation was solved, enabling efficient EFP forming and stable flight, and enhancing its destructive power.

CN118548758BActive Publication Date: 2026-11-20XIAN MODERN CONTROL TECH RES INST
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410808539.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2026-11-20
Estimated Expiration
2044-06-21

AI Technical Summary

Technical Problem

Existing EFP shaped charges are prone to necking and fracture during detonation, affecting the forming of high aspect ratio charges and flight stability, thus limiting the improvement of destructive power.

Method used

By adopting a propellant liner design with gradually changing mechanical properties, and through heterogeneous materials and heat treatment or powder metallurgy technology, the strength and plasticity of the propellant liner are distributed in a radial or axial gradient, forming high-strength regions, transition regions and high-plasticity regions, thus optimizing the EFP molding process.

Benefits of technology

The improved length-to-diameter ratio and destructive power of the EFP ensured that the projectile was less prone to breakage during detonation, enhancing flight stability and the ability to strike armored targets.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118548758B_ABST
    Figure CN118548758B_ABST
Patent Text Reader

Abstract

The present application provides a liner for realizing precise forming of EFP by mechanical property gradient, mainly solves the problem that EFP is easy to neck and then break into two parts under the condition of large length-diameter ratio stretching caused by the influence of high temperature, high pressure and high strain rate of the liner in the blasting process. The present application controls the material property distribution of the plasticity and strength of the liner as needed, so that the liner has the characteristics of mechanical property gradient in the specified direction, realizes the precise strengthening of the "weak place" of EFP forming, and further improves the length-diameter ratio and power of EFP, breaks through the restriction of the existing liner material and explosive performance, provides a new idea for the design of large length-diameter ratio EFP, and further improves the length-diameter ratio of EFP.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of warhead technology of ammunition, specifically relating to a shaped charge liner that achieves precise EFP forming through gradual changes in mechanical properties. Background Technology

[0002] Explosively Formed Projectiles (EFPs) are accelerated and tumbled by a metal shaped charge under the detonation of an explosive charge. The shaped charge is typically a spherical cap, conical, or a combination of curves. They rely on their own kinetic energy to fly long distances and attack targets from above. Due to their insensitivity to altitude and significant after-target effects, they are widely used in terminally guided munitions, top-attack missiles, loitering munitions, and unattended munition systems, and are the primary destructive element of top-attack anti-armor smart munitions.

[0003] Based on the damage mechanism of EFP (Explosive Formed Projectile) against targets, the core technology in this field is how to form a compact, elongated, high-speed projectile with good flight stability. The key to solving this problem lies in controlling parameters such as the length, shape, and mass of the formed projectile, with the shaped charge liner being a crucial influencing factor. The material properties of the shaped charge liner directly affect the projectile's explosive forming process and its destructive power. To improve the ability of EFPs to strike armored targets, higher-density, more resilient metal shaped charge liner materials are used. Precise matching of the warhead explosive charge with the shaped charge liner achieves higher flight speeds and superior aerodynamic shapes, thereby improving the length-to-diameter ratio and flight stability of the EFP. Figure 1 As shown, the existing shaped charge liner is affected by the high temperature, high pressure and high strain rate of the detonation process. The forming shape of the EFP is quite sensitive to the changes in the structure of the shaped charge liner. Under the stretching condition of large length-diameter ratio, the EFP is prone to necking and then breaking into two parts, which seriously restricts the forming of the EFP with a large length-diameter ratio and stable flight, and affects the improvement of the destructive power of the warhead. Summary of the Invention

[0004] To overcome the shortcomings of existing technologies, this invention provides a propellant liner that achieves precise EFP molding through gradual changes in mechanical properties. By utilizing the gradual distribution of mechanical properties such as strength and plasticity of the heterogeneous propellant liner, the "weak points" in EFP molding are precisely strengthened, thereby achieving reliable molding of EFP with a large aspect ratio and increased power.

[0005] The technical solution adopted by this invention to solve its technical problem is as follows:

[0006] A propellant liner for precise EFP molding achieved through gradual changes in mechanical properties is disclosed. The propellant liner is a surface of revolution. The cross-section formed by the edge of the propellant liner is circular. The cross-section formed by the edge of the propellant liner is the bottom surface of the propellant liner. The radius of the bottom surface of the propellant liner is R3. The line connecting the center of the bottom surface of the propellant liner and the vertex of the propellant liner is perpendicular to the bottom surface of the propellant liner. The propellant liner surface is divided into three regions using circles C1 and C2 parallel to the bottom surface of the propellant liner. The radius of C2 is R2, the radius of C1 is R1, and R3>R2>R1. The propellant liner surface region between C1 and C2 is a transition region. The propellant liner surface region between C1 and the vertex of the propellant liner is a high-strength region. The propellant liner surface region between C2 and the bottom surface of the propellant liner is a high-plasticity region.

[0007] The ratio of the area of ​​the high-intensity region to the total area of ​​the liner is S. FIT S FIT The range is 4% ≤ S FIT ≤16%.

[0008] The ratio of the area of ​​the highly plastic region to the total area of ​​the liner is S. PLAS S PLAS The range is: S PLAS ≥36%.

[0009] The strength difference between the high-strength region and the high-plasticity region of the shaped charge liner is not less than 30 MPa.

[0010] The difference in elongation between the high-strength region and the high-plasticity region of the shaped charge liner is ≥10%.

[0011] The shape of the rotating surface of the drug-shaped cover is eccentric sub-hemispherical, conical, arc-conical combined, spherical or eccentric sub-hemispherical.

[0012] The material of the shaped charge shroud is a single metal or an alloy metal.

[0013] The method for forming a shaped charge liner made of a single metal is as follows: a preform material with a gradient grain structure is prepared by non-equilibrium solidification, and the local or surface structure of the preform material is treated by heat treatment to form a structure with a gradient along the radial or axial direction, thereby obtaining a shaped charge liner with a gradient along the radial or axial direction.

[0014] The forming method for the shaped charge liner made of alloy metal is as follows: by powder metallurgy, a blank material with a material composition that varies radially or axially is formed; by forming technology, residual defects in powder metallurgy are eliminated, and uniform and symmetrical distribution of the composition is achieved during the deformation process, thereby obtaining a shaped charge liner with radial gradient composition.

[0015] The elemental metal is copper or pure tantalum; the alloy material is a tantalum-tungsten alloy.

[0016] The beneficial effects of this invention are:

[0017] (1) The present invention provides a propellant liner that achieves precise EFP molding through gradual mechanical property changes. By using the toughening and other gradient control technology, the plasticity and strength distribution of the propellant liner can be controlled as needed, so that the propellant liner has the characteristics of gradual mechanical property changes in a specified direction, which can further improve the length-to-diameter ratio and destructive power of EFP.

[0018] (2) This invention breaks through the constraints of traditional liner materials and explosive properties. It adds a new dimension of material design / control on the basis of existing EFP liner structure design, improves the freedom of warhead design, and helps to control EFP forming.

[0019] (3) The shaped charge shroud of the present invention can adopt different structures such as conical, arc-conical combination, spherical, and eccentric sub-hemispherical, which facilitates the engineering promotion and replacement of existing shaped charge shroud structures and has a wide range of application prospects. Attached Figure Description

[0020] Figure 1 A schematic diagram of necking fracture of a homogeneous drug liner with a large aspect ratio EFP.

[0021] Figure 2 A schematic diagram of the formation process of an EFP (Enhanced Propellant Formation Packet) driven by detonation.

[0022] Figure 3 Schematic diagram of a propellant liner with gradually changing mechanical properties; Figure 3 In the image, (a) is a top view of a shaped charge liner with gradually changing mechanical properties; (b) is a side view of a shaped charge liner with gradually changing mechanical properties; and (c) is a perspective view of a shaped charge liner with gradually changing mechanical properties.

[0023] Figure 4 A schematic diagram illustrating the technical approach for gradient treatment of the mechanical properties of drug-formed liner; Figure 4 In the diagram, (a) is a schematic diagram of a gradient gradient organizational structure design; (b) is a schematic diagram of a gradient gradient component design.

[0024] Figure 5 It is a blank for a drug-shaped casing with gradually changing mechanical properties; Figure 5 In the image, (a) represents a gradient-gradient feature; (b) represents a traditional homogeneous feature.

[0025] Figure 6 This is a diagram of the EFP forming state obtained from pulsed X-ray imaging experiments. Figure 6 In the image, (a) is a gradient-varying drug liner; (b) is a traditional homogeneous drug liner.

[0026] Figure 7Here are schematic diagrams of the configurations of the gradually changing shaped charge shrouds with varying structural mechanical properties; (a) is an arc-cone combined shroud; (b) is a conical shroud; (c) is a spherical cap shroud.

[0027] In the diagram, 1 represents the high-strength region; 2 represents the transition region; and 3 represents the high-plasticity region. Detailed Implementation

[0028] The technical solution adopted by this invention to solve its technical problem is a propellant cover that achieves precise EFP molding through gradual changes in mechanical properties. The propellant cover is a curved surface of revolution; the cross-section formed by the edge of the propellant cover is circular; the cross-section formed by the edge of the propellant cover is the bottom surface of the propellant cover; the radius of the bottom surface of the propellant cover is R3; the line connecting the center of the bottom surface of the propellant cover and the vertex of the propellant cover is perpendicular to the bottom surface of the propellant cover; the curved surface of the propellant cover is divided into three regions using circles C1 and C2 parallel to the bottom surface of the propellant cover; wherein the radius of C2 is R2, the radius of C1 is R1, and R3>R2>R1; the curved surface region of the propellant cover between C1 and C2 is a transition region; the curved surface region of the propellant cover between C1 and the vertex of the propellant cover is a high-strength region; and the curved surface region of the propellant cover between C2 and the bottom surface of the propellant cover is a high-plasticity region.

[0029] The ratio of the area of ​​the high-intensity region to the total area of ​​the liner is S. FIT S FIT The range is 4% ≤ S FIT ≤16%;

[0030] The ratio of the area of ​​the highly plastic region to the total area of ​​the liner is S. PLAS S PLAS The range is S PLAS ≥36%;

[0031] The strength difference between the high-strength region and the high-plasticity region of the shaped charge liner is not less than 30 MPa;

[0032] The difference in elongation between the high-strength region and the high-plasticity region of the shaped charge liner is ≥10%;

[0033] The shape of the drug-formed shroud is eccentric subhemispherical, conical, arc-conical combined, spherical, or eccentric subhemispherical;

[0034] The material of the shaped charge shroud is a single metal or an alloy metal;

[0035] The method for forming a shaped charge liner made of a single metal is as follows: a preform material with a gradient change in grain structure is prepared by non-equilibrium solidification, and the local or surface structure of the preform material is treated by heat treatment to form a shaped charge liner with a gradient change in structure along the radial or axial direction.

[0036] The method for forming a shaped charge liner made of an alloy metal is as follows: a blank material with a radial or axial composition is formed by powder metallurgy; residual defects in the powder metallurgy are eliminated by forming technology to achieve uniform and symmetrical distribution of the composition during deformation, thereby obtaining a shaped charge liner with radial gradient composition.

[0037] The elemental metal is copper or pure tantalum; the alloy material is a tantalum-tungsten alloy.

[0038] The present invention will be further described below with reference to the accompanying drawings and embodiments.

[0039] After detonation, a shaped charge liner precisely formed using EFP (Expanded Forming Material) through gradual changes in mechanical properties collapses, flips, and undergoes axial tensile deformation under the detonation pressure and products of the high-energy explosive. Based on the gradual changes in the shaped charge liner's mechanical properties, a high-strength, dense head, a plastically stretched tail skirt or fin, and a projectile waist with moderate strength and plasticity to prevent necking fracture are formed. Figure 2 As shown;

[0040] like Figure 3-6 As shown, this invention provides a technical solution: a propellant liner that achieves precise EFP molding through gradual changes in mechanical properties. The propellant liner employs... Figure 3 The eccentric sub-hemispherical configuration shown has a shroud diameter R3 of 63 mm, a shroud top height of 14.56 mm, a radius of curvature of 64.86 mm, and a shroud thickness of 4.48 mm. The high-strength region of the shroud, with a diameter R1 approximately 20% of the shroud diameter R3 and an area proportion of approximately 4%, is used to form a high-strength, dense head. The minimum diameter R2 of the high-plasticity region is approximately 80% of the shroud diameter R3 and an area proportion of approximately 36%, used for the plastically stretched tail skirt (or tail fin). The transition region 2, with an area proportion of 60%, possesses moderate strength and plasticity, avoiding material instability and necking fracture caused by sudden changes in mechanical properties, and is used to form the projectile waist. Figure 7 As shown, commonly used shaped charge liner configurations with gradually changing structural mechanical properties include arc-cone combined liner, conical liner, and spherical cap liner;

[0041] To achieve the gradient change in the strong plasticity of the drug-formed liner, the main methods are as follows: Figure 4 The two technical approaches shown are:

[0042] 1) For elemental propellant liner materials such as copper and pure tantalum, the mechanical properties (strength, plasticity, etc.) of the propellant liner can be gradually varied through gradient changes in microstructure. A preform material with a gradient grain structure is prepared through non-equilibrium solidification. The overall or surface strength and toughness of the propellant liner can be controlled through overall deformation or surface deformation. Heat treatment further optimizes the local or surface microstructure of the material, thereby obtaining a gradient microstructure along the radial or axial direction.

[0043] 2) For alloy-type propellant liner with adjustable composition, the mechanical properties (strength, plasticity, etc.) of the propellant liner can be gradually varied through compositional gradient changes. Powder metallurgy is used to form a preform material with radial or axial compositional variations. Forming techniques are then used to eliminate residual defects in the powder metallurgy process, achieving a uniform and symmetrical axial distribution of composition during deformation, thus obtaining a radial gradient composition. Alternatively, surface carburizing / nitriding treatments can be used to further optimize the axial gradient properties.

[0044] In this embodiment, the shaped charge liner is based on T2 copper. The surface of the forged shaped charge liner billet is heat-treated using induction coil heating at a power of 40kW for 1 minute. Under the skin effect, the microstructure of the shaped charge liner billet is gradient-controlled, thereby obtaining the desired microstructure. Figure 5 (a) shows a gradient microstructure that gradually changes radially, and a graded propellant liner with high strength at the center and good plasticity at the edges is formed by machining. Measurements show that the strength difference of the propellant liner is approximately 30 MPa, and the elongation difference is ≥10%.

[0045] Pulsed X-ray imaging experiments were used to test the detonation-driven EFPs formed by a conventional homogeneous copper liner and a copper liner with gradually varying mechanical properties, both with the same structural dimensions. The forming states of the two EFPs at 150 μs were obtained, such as... Figure 6 As shown, both types of EFPs formed by the shaped charge liner are fully stretched, exhibiting fragmented spalling rings, and have similar overall configurations. The EFP formed by the mechanically graded shaped charge liner shows more pronounced collapse at the head compared to the EFP formed by the traditional homogeneous shaped charge liner, resulting in a longer projectile and a more uniform transition. The projectile length increased from 49.59 mm to 55.93 mm, an increase of approximately 12.78%. Furthermore, due to the plasticity advantage at the edge of the graded shaped charge liner, the EFP's tail forms a large-angle tail skirt conducive to stable flight. Penetration tests on a 45# steel target showed that the penetration depth increased from 33.6 mm to 41.3 mm, representing a 22.92% increase in power.

Claims

1. A propellant liner that achieves precise EFP molding through gradual changes in mechanical properties, characterized in that: The shaped charge cover is a curved surface of revolution; the cross-section formed by the edge of the shaped charge cover is circular; the cross-section formed by the edge of the shaped charge cover is the bottom surface of the shaped charge cover; the radius of the bottom surface of the shaped charge cover is... The line connecting the center of the bottom surface of the shaped charge liner and the apex of the shaped charge liner is perpendicular to the bottom surface of the shaped charge liner; a circle parallel to the bottom surface of the shaped charge liner is used. and The curved surface of the drug-formed liner is divided into three regions; among which... The radius is , The radius is , The and The curved surface area of ​​the drug-shaped cover between them is a transition area; the The curved surface region of the propellant liner between the apex and the apex of the propellant liner is a high-intensity region; The curved area of ​​the propellant cover, which is adjacent to the bottom surface of the propellant cover, is a highly plastic area.

2. The shaped charge liner for precise EFP molding achieved through gradual changes in mechanical properties according to claim 1, characterized in that: The ratio of the area of ​​the high-intensity region to the total area of ​​the liner is ; The range is .

3. The shaped charge liner for precise EFP molding achieved through gradual changes in mechanical properties according to claim 1, characterized in that: The ratio of the area of ​​the highly plastic region to the total area of ​​the liner is ; The scope is: .

4. A propellant liner for precise EFP molding achieved through gradual changes in mechanical properties according to claim 1, characterized in that: The strength difference between the high-strength region and the high-plasticity region of the shaped charge liner is not less than 30 MPa.

5. A shaped charge liner for precise EFP molding achieved through gradual changes in mechanical properties according to claim 1, characterized in that: The difference in elongation between the high-strength region and the high-plasticity region of the shaped charge liner is ≥10%.

6. A propellant liner for precise EFP molding achieved through gradual changes in mechanical properties according to claim 1, characterized in that: The shape of the rotating surface of the drug-shaped cover is eccentric sub-hemispherical, conical, arc-conical combined, spherical or eccentric sub-hemispherical.

7. A shaped charge liner for precise EFP molding achieved through gradual changes in mechanical properties according to claim 1, characterized in that: The material of the shaped charge shroud is a single metal or an alloy metal.

8. A shaped charge liner for precise EFP molding achieved through gradual changes in mechanical properties, as described in claim 7, characterized in that: The method for forming a shaped charge liner made of a single metal is as follows: a preform material with a gradient grain structure is prepared by non-equilibrium solidification, and the local or surface structure of the preform material is treated by heat treatment to form a structure with a gradient along the radial or axial direction, thereby obtaining a shaped charge liner with a gradient along the radial or axial direction.

9. A shaped charge liner for precise EFP molding achieved through gradual changes in mechanical properties, as described in claim 7, characterized in that: The forming method for the shaped charge liner made of alloy metal is as follows: by powder metallurgy, a blank material with a material composition that varies radially or axially is formed; by forming technology, residual defects in powder metallurgy are eliminated, and uniform and symmetrical distribution of the composition is achieved during the deformation process, thereby obtaining a shaped charge liner with radial gradient composition.

10. A propellant liner for precise EFP molding achieved through gradual changes in mechanical properties, as described in claim 7, characterized in that: The elemental metal is copper or pure tantalum; the alloy metal is a tantalum-tungsten alloy.

Citation Information

Patent Citations

  • Laser net near forming TiB2 / Ti-based functionally graded material and preparation method thereof

    CN117066529A

  • Large aperture perforating bullet

    CN207847604U