Preparation method of high-strength wear-resistant isotropic pyrolytic carbon
By controlling the microstructure of pyrolytic carbon through hierarchical residence chemical vapor deposition technology, a three-dimensional network structure is formed, which solves the problem of unstable performance of pyrolytic carbon, improves its high strength and wear resistance, and expands its application in biomedicine, aerospace and nuclear industry.
Patent Information
- Application Number
- CN202410588007.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-13
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-05-13
AI Technical Summary
Existing technologies make it difficult to precisely control the microstructure of isotropic pyrolytic carbon, resulting in unstable macroscopic mechanical and tribological properties, which limits its application in fields such as biomedicine, aerospace, and nuclear industry.
By employing a staged residence chemical vapor deposition technique, and by adjusting process parameters such as graphite mold size, carbon source gas flow rate, deposition system pressure, and temperature, an interpenetrating structure of carbon nanospheres and sheet graphene is achieved, forming a three-dimensional network structure of high-strength, wear-resistant, isotropic pyrolytic carbon.
It significantly improves the flexural strength and wear resistance of pyrolytic carbon, increases the density to 1.73 g/cm³, achieves a flexural strength of 221.2 MPa, and reduces the wear rate to 8.8 × 10⁻⁶ mm³·N⁻¹·m⁻¹, making it suitable for bone prostheses, engine throat liners, and nuclear fuel coatings.
Smart Images

Figure CN118563276B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of pyrolytic carbon technology, specifically to a high-strength, wear-resistant, isotropic pyrolytic carbon, its preparation method, and its applications. Background Technology
[0002] Pyrolytic carbon is widely used in biomedicine, aerospace, and nuclear industries due to its excellent biocompatibility, abrasion resistance, high-temperature mechanical properties, and high-temperature stability. Based on its microstructure, pyrolytic carbon can generally be divided into anisotropic pyrolytic carbon (rough and smooth layers) and isotropic pyrolytic carbon (IPC). IPC consists of micro- and nano-sized carbon spheres, exhibiting a dense structure, small grain size, and uniform properties. In addition to possessing the common characteristics of general pyrolytic carbon materials, it also features high strength, impermeability, and excellent processability. IPC can be used as a coating material in artificial heart valves and small bone prostheses, and can also be used as a composite coating to encapsulate fission radioactive elements in fuel particles.
[0003] IPC materials are generally prepared by chemical vapor deposition (CVD), using hydrocarbons as raw materials and forming on the surface of a thermal substrate under certain conditions. Those skilled in the art have prepared IPCs with a thickness of approximately 2-5 mm at 1400-1500℃ using propane as the carbon source, argon and hydrogen as dilution and carrier gases, hollow alumina spheres as bed particles, and graphite as the substrate. The density of the prepared IPCs was approximately 1.70-1.93 g / cm³. 3 The carbon spheres have a diameter of approximately 300 nm to 2 μm, and are connected by sheet-like graphite layers, achieving a flexural strength of up to 166 MPa. Meanwhile, those skilled in the art have also prepared boron-doped IPCs using methane and BCl4 at 1250 °C. Studies have shown that boron can improve the growth efficiency of IPCs without damaging their structure, but the effect on their mechanical properties has not been investigated. Those skilled in the art have also prepared IPCs using methane as the carbon source and graphite tubes as the substrate at 1000-1050 °C, finding that with increasing temperature, the density of IPCs decreases, the porosity increases, and the coefficient of thermal expansion does not change significantly. Those skilled in the art have also prepared carbon fibers with an inner layer of IPC and an outer layer of low-texture carbon at 900 °C using propylene as the carbon source and hydrogen as the carrier gas. The IPC structure consists of irregular spherical grains, each composed of an outer medium-texture graphite layer and an inner dense carbon nanoparticle layer, resulting in fibers with excellent isotropic mechanical properties. Those skilled in the art used propylene as the carbon source and hydrogen and argon as diluent gases to prepare IPCs on graphite disks at 1550°C by guiding the gas through a graphite column. The density of the IPCs was approximately 1.72 g / cm³. 3The carbon particles are approximately 1-2 μm in size. Tribological tests revealed that increasing the thickness of the graphite flakes on the outer layer of the carbon particles can effectively improve the stability of the friction coefficient, increase the hardness of the IPC, and thus reduce its wear rate.
[0004] Current reports on intercellular carbon (IPC) are limited to preparation and simple performance testing, with limited research on its mechanisms and structural control. With the development of biomedicine and advanced technologies, more stringent requirements are being placed on controlling and optimizing the mechanical and tribological properties of IPC. Generally, reducing the size of carbon nanospheres can improve the mechanical properties of IPC. However, simply reducing the size of the carbon nanospheres leads to the formation of numerous grain boundaries and weak interfacial bonding. Under actual load-bearing conditions, this accelerates crack propagation along these defects, exacerbating the instability of macroscopic mechanical properties, reducing its macroscopic tribological performance, and limiting its applications. The microstructure of IPC can be divided into a dense carbon particle core and a graphite sheet shell. The carbon particle core has an onion-like graphite sheet structure, while the interconnected outer graphite sheets give the material isotropic properties. Therefore, the performance of IPC is mainly determined by the size and distribution of the core carbon particles, the size and thickness of the outer graphite sheets, and the overall density and porosity of the material. Precise control and optimization of the microstructure of IPC is crucial to its macroscopic performance. Summary of the Invention
[0005] To address the shortcomings of the aforementioned background technologies, this invention provides a high-strength, wear-resistant, isotropic pyrolytic carbon, its preparation method, and its applications. This invention allows for precise control of the microstructure of IPCs, employs a simple preparation method with a short cycle time and low cost, and is of significant importance in fields such as biomedicine, high-temperature thermal protection, and load-bearing applications.
[0006] The first objective of this invention is to provide a method for preparing high-strength, wear-resistant, isotropic pyrolytic carbon, comprising the following steps: Graphite rods and graphite columns are placed sequentially in the deposition furnace along the direction in which the carbon source is introduced; The diameter ratio of the graphite rod to the graphite column is 1 to 3:4; the graphite column is located in the heating zone of the deposition furnace. The deposition furnace is evacuated and heated to 900~1200℃. Methane gas is then introduced into the deposition furnace as a carbon source. After deposition for 2~50 hours, pyrolytic carbon with carbon nanospheres encapsulated in a three-dimensional network of graphene is obtained.
[0007] Preferably, the diameter of the graphite column is less than 10 mm compared to the inner diameter of the heating zone in the deposition furnace.
[0008] Preferably, the flow rate of the methane gas introduced is 100~500 ml / min.
[0009] Preferably, after introducing methane gas, the pressure inside the deposition furnace is adjusted to 10~500 mbar by adjusting the vacuum pump. The graphite rod guides the carbon source to the graphite column, allowing the pyrolytic carbon to be adsorbed and grown on the graphite column.
[0010] Preferably, after deposition is completed, heating is stopped and the flow of methane is shut off. After the deposition furnace cools to room temperature, argon gas is introduced to bring the pressure inside the deposition furnace close to atmospheric pressure.
[0011] The second objective of this invention is to provide a high-strength, wear-resistant, isotropic pyrolytic carbon.
[0012] The third objective of this invention is to provide an application of high-strength, wear-resistant, isotropic pyrolytic carbon in bone prostheses, engine throat liners, or nuclear fuel coatings.
[0013] Compared with the prior art, the beneficial effects of the present invention are: This invention provides a high-strength, wear-resistant, isotropic pyrolytic carbon, its preparation method, and its applications. By changing the size of a graphite mold and using only methane as the carbon source gas, this invention precisely controls the microstructure of the prepared IPC (integrated carbon polymerate) at low temperatures by adjusting the methane flow rate and system pressure. By designing and changing the size of the graphite mold, this invention alters the carbon source gas flow field and achieves partitioned retention, dividing the IPC deposition and growth into two stages to achieve gradient carbon pyrolysis and adsorption. This invention employs a staged residence chemical vapor deposition (CVD) technique. By adjusting process parameters such as the size of the graphite mold, the carbon source gas flow rate, the deposition system pressure, time, and temperature, precise control of the interpenetrating structure of carbon nanospheres and sheet graphene in the IPC can be achieved, thereby improving macroscopic mechanical and tribological properties. In this invention, methane pyrolysis forms polycyclic aromatic hydrocarbons, which then form carbon clusters. If the methane concentration is too low, the carbon atom clusters formed by pyrolysis are small and flat, making them difficult to twist and bend. When the methane concentration is appropriate, it can produce carbon structures with fewer defects, forming twisted carbon clusters with optimal proportions, and subsequently forming nanoscale carbon spheres. When the reaction time is short, methane cracking produces small, flat polycyclic aromatic hydrocarbons (PAHs), which are rapidly adsorbed onto the mold, forming larger, ordered, multilayered graphene sheets. When the reaction time is long, the PAHs are twisted and adsorbed, making it difficult to unfold and form particles. Therefore, changing the gas reaction time can regulate the size and morphology of the PAHs formed by the gas pyrolysis carbon reaction. When the size of the PAHs further increases, they can be rapidly adsorbed onto the graphene substrate, and the morphology of the PAHs significantly affects the deposition results. Therefore, a longer reaction time helps form curved, cross-linked nanosphere carbon particles, while a shorter reaction time helps form ordered graphene sheet structures. Furthermore, due to the template effect caused by the carbon spheres, the graphene sheet structure is highly cross-linked and curves around the carbon spheres, but tends to align parallel to the carbon spheres, thus growing and encapsulating them to form a three-dimensional network structure. When the ratio of carbon spheres to graphene is small, the template effect of the carbon spheres weakens, tending to form a more regular and isotropic pyrolytic carbon structure. When the ratio of carbon spheres to graphene is too large, the graphite sheets are small, the bonding with the carbon spheres is weak, and the cross-linking structure cannot be achieved, significantly reducing the mechanical properties of IPC. When the carbon sphere ratio is appropriate, sheet-like graphene can effectively increase the compactness of the three-dimensional network structure, improve the load-bearing and transporting capacity of the graphene sheets, and thus significantly improve the mechanical properties of IPC. Therefore, the construction of the microstructure of high-strength IPC must first form carbon sphere particles of a certain size and content, and then grow sheet-like graphene to cross-link with the carbon sphere particles to form a three-dimensional network structure. Therefore, this invention relates to a hierarchical residence chemical vapor deposition technique, which, through mold design, achieves hierarchical preparation and cross-linking interpenetration of carbon sphere particles and graphene sheet structures.
[0014] Therefore, the strength of the IPC prepared in this invention depends on its microstructure, and the formation of the microstructure depends on the reaction temperature, time, methane concentration, and deposition system pressure. In this invention, the formation rate, content, and size of the carbon spheres are comprehensively determined by the reaction time and methane concentration; the size, content, and adsorption rate of the graphene sheets are mainly determined by the reaction time and deposition system pressure. Therefore, by adjusting the temperature, methane concentration, and graphite mold size, the key reaction time, reaction temperature, and gas flow rate required for the formation of carbon spheres can be effectively adjusted. Adjusting the temperature, methane concentration, gas flow rate, and deposition system pressure can effectively adjust the reaction time and reaction temperature required for the formation of the three-dimensional graphene structure, thereby adjusting the ratio of graphene sheets to carbon spheres and the structure, achieving controllable adjustment of its mechanical properties. By adjusting the preparation parameters and optimizing the microstructure, the IPC prepared in this invention has a thickness of 1-5 mm and a density of approximately 1.73 g / cm³. 3 With an open area ratio as low as 0.16%, a flexural strength of 221.2 MPa (approximately 33.25% higher than the reported IPC flexural strength), and a flexural modulus of 27.16 GPa, the wear rate measured under a 20 N load using silicon carbide balls as the friction pair was only 8.8 × 10⁻⁶. -6 mm 3 ·N -1 ·m -1 This invention provides a new approach for the CVD preparation of pyrolytic carbon materials, and the prepared IPCs possess excellent and tunable mechanical and tribological properties, which is of great significance in fields such as biomedicine, aerospace, and nuclear industry. Attached Figure Description
[0015] Figure 1 This is a schematic diagram of the IPC preparation process; Figure 2 A scanning electron microscope image of the IPC prepared in Example 1; Figure 3 A transmission electron microscope image of the IPC prepared in Example 1; Figure 4 The image shows a scanning electron microscope image of the IPC prepared in Example 2. Detailed Implementation
[0016] To enable those skilled in the art to better understand and implement the technical solutions of the present invention, the present invention will be further described below in conjunction with specific embodiments and accompanying drawings. However, the embodiments described are not intended to limit the present invention.
[0017] This invention presents a novel staged residence-based chemical vapor deposition (IPC) method. By altering the gas flow field in the staged gas path, the reaction region is divided into a long residence-area reaction zone (LRRA) and a short residence-area reaction zone (SRRA). In the LRRA, methane undergoes thorough pyrolysis and polymerization to form coiled structures and carbon nanospheres, which are then carried to the SRRA by eddies created by the carbon source gas flow field. The size and number of carbon nanospheres generated are adjusted by regulating the methane flow rate, system pressure, deposition temperature, and the size of the LRRA. In the SRRA, carbon nanospheres are adsorbed onto graphite pillars, and the carbon source gas decomposes to form graphene sheets that grow on the surface of the carbon nanospheres and encapsulate them. Furthermore, due to the high flow rate and temperature of the carbon source gas, the graphene sheets grow rapidly to form large-sized sheets, creating an interpenetrating structure with the carbon nanospheres. This interpenetrating structure allows the IPC to effectively transfer the load to the carbon nanospheres during operation, significantly improving the mechanical strength and tribological properties of the IPC. This invention enables precise control and optimization of the microstructure of IPC by adjusting the reaction time, temperature, and gas flow rate during preparation, thereby producing high-strength and wear-resistant IPC.
[0018] The first aspect of this invention provides a method for preparing high-strength, wear-resistant, isotropic pyrolytic carbon, comprising the following steps: Graphite rods and graphite columns are placed sequentially in the deposition furnace along the direction in which the carbon source is introduced; The diameter ratio of the graphite rod to the graphite column is 1 to 3:4; the graphite column is located in the heating zone of the deposition furnace. The deposition furnace is evacuated and heated to 900~1200℃. Methane gas is then introduced into the deposition furnace as a carbon source. After deposition for 2~50 hours, pyrolytic carbon with carbon nanospheres encapsulated in a three-dimensional network of graphene is obtained.
[0019] It should be noted that, see Figure 1 As shown, graphite rods and graphite columns are placed sequentially in the deposition furnace along the direction of carbon source introduction. That is, the graphite rods and graphite columns are combined to form a T-shaped structure, and the graphite columns are completely in the heating zone of the furnace. Methane gas is introduced into the furnace as a carbon source, and the graphite rods guide the carbon source to the graphite columns, so that the pyrolytic carbon is adsorbed and grows on the graphite columns.
[0020] The diameter of the graphite column is less than 10 mm compared to the inner diameter of the heating zone in the deposition furnace.
[0021] The flow rate of methane gas introduced is 100~500 ml / min.
[0022] After introducing methane gas, the pressure inside the deposition furnace is adjusted to 10~500 mbar by adjusting the vacuum pump. The graphite rod guides the carbon source to the graphite column, allowing the pyrolytic carbon to be adsorbed and grown on the graphite column.
[0023] After deposition is complete, heating is stopped and the flow of methane is shut off. Once the deposition furnace has cooled to room temperature, argon gas is introduced to bring the pressure inside the furnace close to atmospheric pressure.
[0024] In one embodiment, a method for preparing high-strength, wear-resistant, isotropic pyrolytic carbon includes the following steps: The chemical vapor deposition (CVD) process is used to place graphite rods and graphite columns into a CVD furnace. The graphite rods and graphite columns are combined to form a T-shaped structure, so that the graphite column is completely in the heating zone of the furnace. The diameter ratio of the graphite rod to the graphite column is 1:4 to 3:4. The diameter of the graphite column is 10 mm smaller than the inner diameter of the heating zone of the furnace. The axes of the graphite rod, the graphite column and the deposition furnace are completely parallel.
[0025] The deposition system was evacuated, and evacuation was stopped when the pressure inside the furnace reached 2 mbar. Under vacuum, the temperature inside the deposition furnace was raised to 900–1200 °C. Methane gas was introduced into the furnace as a carbon source at a flow rate of 100–500 ml / min, and the system pressure was adjusted to 10–500 mbar by the vacuum pump. Graphite rods guided the carbon source to the graphite columns, allowing pyrolytic carbon to adsorb and grow on the graphite columns. After deposition for 2–50 hours, heating was stopped and the methane flow was shut off. After cooling to room temperature, argon gas was introduced to bring the furnace pressure close to atmospheric pressure. The resulting IPC (Integrated Polymer Carbon) with carbon nanospheres encapsulated in a three-dimensional graphene network was then obtained.
[0026] A second aspect of the present invention provides a high-strength, wear-resistant, isotropic pyrolytic carbon.
[0027] A third aspect of the present invention provides the application of high-strength, wear-resistant, isotropic pyrolytic carbon in bone prostheses, engine throat liners, or nuclear fuel coatings.
[0028] It should be noted that, unless otherwise specified, the experimental methods used in this invention are all conventional methods; and the reagents and materials used, unless otherwise specified, are all commercially available.
[0029] Example 1 A method for preparing high-strength, wear-resistant, isotropic pyrolytic carbon includes the following steps: The chemical vapor deposition (CVD) process is used to place graphite rods and graphite columns into a CVD furnace. The graphite rods and graphite columns are combined to form a T-shaped structure, so that the graphite column is completely in the heating zone of the furnace. The diameter ratio of the graphite rod to the graphite column is 1:4, and the diameter of the graphite column is 10mm smaller than the inner diameter of the heating zone of the furnace.
[0030] The deposition system was evacuated, and the evacuation was stopped when the pressure inside the furnace reached 2 mbar. Under vacuum, the temperature inside the deposition furnace was raised to 900°C. Methane gas was introduced into the furnace as a carbon source at a flow rate of 100 ml / min, and the system pressure was adjusted to 10 mbar. Graphite rods guided the carbon source to the graphite columns, allowing pyrolytic carbon to adsorb and grow on the graphite columns. After 10 hours of deposition, heating was stopped and the methane flow was shut off. After cooling to room temperature, argon gas was introduced to bring the furnace pressure close to atmospheric pressure. The resulting IPC (Integrated Polymer Carbon) was obtained by removing the carbon nanospheres encapsulated in a three-dimensional graphene network.
[0031] Scanning electron microscope image of the IPC prepared in Example 1, see... Figure 2 Carbon nanospheres are uniformly coated with graphene, forming a three-dimensional network structure. (See transmission electron microscope image). Figure 3 Further observation revealed that nanoscale carbon particles were encapsulated by curved, layered graphene sheets, with adjacent particles being encapsulated and cross-linked within the same sheet, forming an interpenetrating structure. The density of the IPC prepared in this example was approximately 1.73 g / cm³. 3 The porosity is approximately 0.16%, and the flexural strength and flexural modulus are 221.2 MPa and 27.16 GPa, respectively. Using silicon carbide balls as the friction pair, the wear rate was measured to be only 8.8 × 10⁻⁶ under a load of 20 N. - 6 mm 3 ·N -1 ·m -1 It possesses excellent mechanical strength and resistance to friction and wear.
[0032] Example 2 A method for preparing high-strength, wear-resistant, isotropic pyrolytic carbon includes the following steps: The chemical vapor deposition (CVD) process is used to place graphite rods and graphite columns into a CVD furnace. The graphite rods and graphite columns are combined to form a T-shaped structure, so that the graphite column is completely in the heating zone of the furnace. The diameter ratio of the graphite rod to the graphite column is 2:4, and the diameter of the graphite column is 10mm smaller than the inner diameter of the heating zone of the furnace.
[0033] The deposition system was evacuated, and the evacuation was stopped when the pressure inside the furnace reached 2 mbar. Under vacuum, the temperature inside the deposition furnace was raised to 1000℃. Methane gas was introduced into the furnace as a carbon source at a flow rate of 200 ml / min, and the system pressure was adjusted to 50 mbar. Graphite rods guided the carbon source to the graphite columns, allowing pyrolytic carbon to adsorb and grow on the graphite columns. After 30 hours of deposition, heating was stopped and the methane flow was shut off. After cooling to room temperature, argon gas was introduced to bring the furnace pressure close to atmospheric pressure. The resulting IPC (Integrated Polymer Carbon) was obtained by removing the material and encapsulating carbon nanospheres with a three-dimensional graphene network.
[0034] Scanning electron microscope image of the IPC prepared in Example 2, see... Figure 3 The carbon nanospheres are uniformly coated with graphene. The spherical particles have a relatively clear morphology but large pores, and a density of approximately 1.73 g / cm³. 3 The porosity is approximately 0.18%, and the flexural strength and flexural modulus are 110.5 MPa and 11.3 GPa, respectively. Using silicon carbide balls as the friction pair, its wear rate was measured to be only 9.8 × 10⁻⁶ under a load of 20 N. -6 mm 3 ·N -1 ·m -1 It possesses good mechanical strength and excellent resistance to friction and wear.
[0035] Comparative Example 1 A method for preparing pyrolytic carbon includes the following steps: The chemical vapor deposition (CVD) process is used to place graphite rods and graphite columns into a CVD furnace. The graphite rods and graphite columns are combined to form a T-shaped structure, so that the graphite column is completely in the heating zone of the furnace. The diameter ratio of the graphite rod to the graphite column is 3.5:4, and the diameter of the graphite column is 10mm smaller than the inner diameter of the heating zone of the furnace.
[0036] The deposition system was evacuated, and the evacuation was stopped when the pressure inside the furnace reached 2 mbar. Under vacuum, the temperature inside the deposition furnace was raised to 1200℃. Methane gas was introduced into the furnace as a carbon source at a flow rate of 500 ml / min, and the system pressure was adjusted to 500 mbar. Graphite rods guided the carbon source to the graphite columns, allowing the pyrolytic carbon to adsorb and grow on the graphite columns. After 40 hours of deposition, heating was stopped and the methane flow was shut off. After cooling to room temperature, argon gas was introduced to bring the furnace pressure close to atmospheric pressure. The resulting IPC (Integrated Polymer Carbon) was obtained by removing the material and encapsulating carbon nanospheres with a three-dimensional graphene network.
[0037] The carbon particles in the IPC prepared using Comparative Example 1 were large in size and had large pores. Due to the excessively large diameter of the grinding rod, the carbon source had a short residence time in the LRRA, resulting in fewer carbon nanospheres formed. The graphene sheet growth rate in the SRRA was too fast, leading to excessively thick graphene sheets and thus large pores. The porosity was approximately 0.34%, resulting in a flexural strength of only 63.7 MPa. Using silicon carbide balls as the friction pair, its wear rate was measured to be 2.5 × 10⁻⁶ under a load of 20 N. -5 mm 3 ·N -1 ·m -1 The bending strength is significantly different from the previously reported bending strength of 166 MPa, and the wear rate is significantly different compared with Examples 1 and 2.
[0038] This invention describes preferred embodiments and their effects. However, those skilled in the art, upon learning the basic inventive concept, can make other changes and modifications to these embodiments. Therefore, the appended claims are intended to include both the preferred embodiments and all changes and modifications falling within the scope of this invention.
[0039] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A method for preparing high-strength, wear-resistant, isotropic pyrolytic carbon, characterized in that, Includes the following steps: Graphite rods and graphite columns are placed sequentially in the deposition furnace along the direction in which the carbon source is introduced; The diameter ratio of the graphite rod to the graphite column is (1~3):4; the graphite column is located in the heating zone of the deposition furnace. The deposition furnace is evacuated and heated to 900~1200℃. Methane gas is then introduced into the deposition furnace as a carbon source. After deposition for 2~50 hours, pyrolytic carbon with carbon nanospheres encapsulated in a three-dimensional network of graphene is obtained.
2. The method for preparing high-strength, wear-resistant, isotropic pyrolytic carbon according to claim 1, characterized in that, The diameter of the graphite column is 10 mm smaller than the inner diameter of the heating zone in the deposition furnace.
3. The method for preparing high-strength, wear-resistant, isotropic pyrolytic carbon according to claim 1, characterized in that, The flow rate of methane gas introduced is 100~500 mL / min.
4. The method for preparing high-strength, wear-resistant, isotropic pyrolytic carbon according to claim 1, characterized in that, After introducing methane gas, the pressure inside the deposition furnace is adjusted to 10~500 mbar by adjusting the vacuum pump. The graphite rod guides the carbon source to the graphite column, allowing the pyrolytic carbon to be adsorbed and grown on the graphite column.
5. The method for preparing high-strength, wear-resistant, isotropic pyrolytic carbon according to claim 1, characterized in that, After deposition is complete, heating is stopped and the flow of methane is shut off. Once the deposition furnace has cooled to room temperature, argon gas is introduced to bring the pressure inside the furnace close to atmospheric pressure.
6. A high-strength, wear-resistant, isotropic pyrolytic carbon prepared by the method according to any one of claims 1 to 5.
7. The application of the high-strength, wear-resistant, isotropic pyrolytic carbon of claim 6 in bone prostheses, engine throat liners, or nuclear fuel coatings.