A method for removing impurities from diamond surfaces based on MPCVD equipment
The graphite and amorphous carbon impurities on the diamond surface are removed through the hydrogen-oxygen plasma etching technology in the MPCVD equipment, which solves the problem of impurity coverage on the diamond surface after MPCVD synthesis and realizes the feasibility of diamond transparency recovery and quality inspection.
Patent Information
- Application Number
- CN202411046608.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-08-01
AI Technical Summary
The surface of single crystal diamond synthesized by MPCVD is covered with impurities such as graphite and amorphous carbon after epitaxial growth, making it impossible to conduct quality inspection and determine whether it is qualified.
The diamond surface is etched using hydrogen-oxygen plasma in MPCVD equipment. Hydrogen-oxygen plasma is generated through different ratios of hydrogen plasma and oxygen plasma. The growth surface and back surface are etched respectively to remove sp2 phase impurities on the surface. .
It effectively removes impurities on the diamond surface and restores its transparent appearance, ensuring the smooth progress of diamond quality inspection.
Smart Images

Figure CN118563278B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of diamond cultivation technology, and in particular to a method, system, terminal and computer-readable storage medium for removing impurities from the surface of diamond based on MPCVD equipment. Background Art
[0002] Diamond has attracted everyone's attention due to its extremely excellent physical and chemical properties. However, the reserves of natural diamond are limited, so people have developed a variety of synthetic diamond methods, such as high temperature and high pressure method (HPHT, High pressure High temperature), hot filament chemical vapor deposition method (HFCVD, hot filament chemical vapor deposition), etc. Among them, the microwave plasma chemical vapor deposition method (MPCVD, Microwave plasma chemical vapor deposition) synthetic diamond method can synthesize high-quality and large-area diamonds without the introduction of impurities. It has the advantages of no electrode discharge pollution, fast deposition rate, good stability, etc., and is considered to be the best method for preparing high-quality single-crystal diamonds.
[0003] However, the surface of the diamond obtained after the epitaxial growth of the single-crystal diamond synthesized by MPCVD (i.e., the upper surface (generally referred to as the growth surface) and the lower surface (generally referred to as the back surface)) is covered with a layer of opaque graphite, amorphous carbon (sp 2 phase) and other impurities, which makes it impossible to conduct quality inspection on the growth of diamonds and determine whether they are qualified.
[0004] Therefore, the prior art still needs to be improved and developed. Summary of the invention
[0005] The main purpose of the present invention is to provide a method, system, terminal and computer-readable storage medium for removing impurities from the surface of diamond based on MPCVD equipment, aiming to solve the problem in the prior art that the surface of the diamond obtained after the epitaxial growth of single-crystal diamond synthesized by MPCVD is covered with a layer of impurities such as opaque graphite and amorphous carbon, thereby making it impossible to perform quality inspection on the growth of the diamond and determine whether it is qualified.
[0006] To achieve the above object, the present invention provides a method for removing impurities from the surface of diamond based on an MPCVD device, and the method for removing impurities from the surface of diamond based on an MPCVD device comprises the following steps:
[0007] When the first etching instruction is received, the reaction chamber where the diamond to be etched is located is vacuumed according to the first etching instruction;
[0008] When the vacuum treatment is completed, hydrogen and oxygen in a preset flow range are filled into the reaction chamber, and the hydrogen and oxygen are subjected to plasma excitation treatment to obtain hydrogen-oxygen plasma;
[0009] Performing a growth surface etching process on the growth surface of the diamond to be etched according to the hydrogen-oxygen plasma to complete the removal of impurities from the growth surface of the diamond to be etched;
[0010] When the growth surface etching process is completed and a second etching instruction is received, hydrogen plasma is obtained according to the second etching instruction, and a back side etching process is performed on the back side of the diamond to be etched according to the hydrogen plasma to complete the removal of impurities on the back side of the diamond to be etched.
[0011] Optionally, the method for removing impurities from the surface of diamond based on MPCVD equipment, wherein when the first etching instruction is received, the reaction chamber where the diamond to be etched is located is vacuumed according to the first etching instruction, specifically comprising:
[0012] Place the diamond to be etched on a molybdenum holder with the growth surface facing upward;
[0013] Placing the molybdenum tray carrying the diamond to be etched on the substrate stage of the reaction chamber of the MPCVD device and performing a sealing process;
[0014] When the first etching instruction sent by the user is received, the MPCVD device is started, and the reaction chamber where the diamond to be etched is located is vacuumed according to the first etching instruction.
[0015] Optionally, in the method for removing impurities from the surface of diamond based on MPCVD equipment, the hydrogen-oxygen plasma comprises hydrogen plasma and oxygen plasma;
[0016] When the vacuuming process is completed, hydrogen and oxygen in a preset flow range are filled into the reaction chamber, and the hydrogen and oxygen are subjected to plasma excitation process to obtain hydrogen-oxygen plasma, which specifically includes:
[0017] When the vacuuming process is completed, hydrogen gas within a first preset flow rate range is filled into the reaction chamber, and the gas pressure in the reaction chamber is monitored in real time;
[0018] When the pressure in the chamber reaches a first preset pressure range, the hydrogen is subjected to plasma excitation treatment to obtain hydrogen plasma, and the growth surface of the diamond to be etched is initially etched according to the hydrogen plasma;
[0019] The reaction chamber is filled with oxygen within a preset flow range, and the oxygen is subjected to plasma excitation treatment to obtain oxygen plasma.
[0020] Optionally, the method for removing impurities from the surface of diamond based on MPCVD equipment, wherein the step of filling the reaction chamber with oxygen in a preset flow range and performing plasma excitation treatment on the oxygen to obtain oxygen plasma, specifically comprises:
[0021] The flow rate of the hydrogen is increased, and when the flow rate of the hydrogen reaches the second preset flow rate range, oxygen within a third preset flow rate range is filled into the reaction chamber;
[0022] Increasing the gas pressure and microwave power in the cavity, and monitoring the surface temperature of the diamond to be etched in real time;
[0023] When the surface temperature reaches a first preset temperature range, the oxygen is subjected to plasma excitation treatment to obtain oxygen plasma.
[0024] Optionally, the method for removing impurities from the surface of diamond based on MPCVD equipment, wherein the growth surface etching treatment is performed on the growth surface of the diamond to be etched according to the hydrogen-oxygen plasma to complete the removal of impurities from the growth surface of the diamond to be etched, specifically includes:
[0025] performing growth surface etching treatment on the growth surface of the diamond to be etched according to the hydrogen plasma and the oxygen plasma, and when the time of the growth surface etching treatment reaches a first preset time range, shutting down the MPCVD device to cool the cavity;
[0026] When the surface temperature of the diamond after the cavity is cooled is consistent with the room temperature, the diamond that has been cooled is taken out from the reaction chamber of the MPCVD equipment, and the growth surface of the diamond to be etched is etched.
[0027] Optionally, the method for removing impurities from the surface of diamond based on MPCVD equipment, wherein when the growth surface etching process is completed and a second etching instruction is received, obtaining hydrogen plasma according to the second etching instruction specifically includes:
[0028] When the growth surface of the diamond to be etched is completely etched, the diamond to be etched is placed on the molybdenum support with the back side facing upward;
[0029] Placing the molybdenum support carrying the diamond to be etched on the substrate table and performing sealing treatment;
[0030] When receiving the second etching instruction from the user, the MPCVD device is started, and a reaction chamber of the MPCVD device is vacuumed;
[0031] When the vacuuming process is completed, hydrogen gas within the first preset flow rate range is filled into the reaction chamber, and the gas pressure in the reaction chamber is monitored in real time;
[0032] When the gas pressure in the cavity is within the first preset gas pressure range, the hydrogen gas is subjected to plasma excitation processing to obtain hydrogen plasma.
[0033] Optionally, the method for removing impurities from the surface of diamond based on MPCVD equipment, wherein the back side etching treatment is performed on the back side of the diamond to be etched according to the hydrogen plasma to complete the removal of impurities from the back side of the diamond to be etched, specifically comprises:
[0034] The flow rate of the hydrogen is increased, and when the flow rate of the hydrogen reaches a fourth preset flow rate range, the gas pressure in the cavity and the microwave power in the cavity are increased, and the surface temperature of the diamond to be etched is monitored in real time;
[0035] When the surface temperature reaches a second preset temperature range, a back side etching process is performed on the back side of the diamond to be etched according to the hydrogen plasma, and when the back side etching process reaches a second preset time range, the MPCVD device is turned off to cool the cavity;
[0036] When the surface temperature of the diamond after the cavity is cooled is consistent with the room temperature, the diamond that has been cooled is taken out from the reaction chamber of the MPCVD equipment, and the back etching of the diamond to be etched is completed.
[0037] In addition, to achieve the above-mentioned purpose, the present invention further provides a diamond surface impurity removal system based on an MPCVD device, wherein the diamond surface impurity removal system based on an MPCVD device comprises:
[0038] A vacuum processing module, for performing a vacuum processing on a reaction chamber where the diamond to be etched is located according to the first etching instruction when receiving the first etching instruction;
[0039] A plasma excitation module, used for filling the reaction chamber with hydrogen and oxygen within a preset flow range when the vacuum treatment is completed, and performing plasma excitation treatment on the hydrogen and oxygen to obtain hydrogen-oxygen plasma;
[0040] A growth surface impurity removal module, used for performing growth surface etching treatment on the growth surface of the diamond to be etched according to the hydrogen-oxygen plasma to complete the removal of impurities from the growth surface of the diamond to be etched;
[0041] The back impurity removal module obtains hydrogen plasma according to the second etching instruction when the growth surface etching process is completed and the second etching instruction is received, and performs back etching process on the back side of the diamond to be etched according to the hydrogen plasma to complete the back impurity removal of the diamond to be etched.
[0042] In addition, to achieve the above-mentioned purpose, the present invention also provides a terminal, wherein the terminal includes: a memory, a processor, and a diamond surface impurity removal program based on MPCVD equipment stored in the memory and executable on the processor, wherein the diamond surface impurity removal program based on MPCVD equipment implements the steps of the diamond surface impurity removal method based on MPCVD equipment as described above when the diamond surface impurity removal program based on MPCVD equipment is executed by the processor.
[0043] In addition, to achieve the above-mentioned purpose, the present invention also provides a computer-readable storage medium, wherein the computer-readable storage medium stores a diamond surface impurity removal program based on MPCVD equipment, and when the diamond surface impurity removal program based on MPCVD equipment is executed by a processor, the steps of the diamond surface impurity removal method based on MPCVD equipment as described above are implemented.
[0044] In the present invention, when a first etching instruction is received, the reaction chamber where the diamond to be etched is located is evacuated according to the first etching instruction; when the evacuation is completed, hydrogen and oxygen in a preset flow range are filled into the reaction chamber, and the hydrogen and oxygen are subjected to plasma excitation to obtain hydrogen-oxygen plasma; the growth surface of the diamond to be etched is etched according to the hydrogen-oxygen plasma to complete the removal of impurities on the growth surface of the diamond to be etched; when the growth surface etching is completed and a second etching instruction is received, hydrogen plasma is obtained according to the second etching instruction, and the back side of the diamond to be etched is etched according to the hydrogen plasma to complete the removal of impurities on the back side of the diamond to be etched. The present invention generates corresponding hydrogen-oxygen plasma by inputting different contents of hydrogen and oxygen, which can respectively realize the effective removal of impurities on the surface of the diamond after epitaxial growth, so that the diamond can restore its transparent appearance and ensure the smooth progress of the diamond quality inspection process. BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 It is a flow chart of a preferred embodiment of the method for removing impurities from the surface of diamond based on MPCVD equipment of the present invention;
[0046] Figure 2It is a schematic diagram of the impurity removal process of the growth surface of the diamond to be etched according to a preferred embodiment of the diamond surface impurity removal method based on MPCVD equipment of the present invention;
[0047] Figure 3 It is a schematic diagram of a process for removing impurities from the back side of a diamond to be etched according to a preferred embodiment of the method for removing impurities from the surface of a diamond based on an MPCVD device of the present invention;
[0048] Figure 4 It is a structural diagram of a preferred embodiment of a diamond surface impurity removal system based on MPCVD equipment of the present invention;
[0049] Figure 5 It is a structural diagram of a preferred embodiment of the terminal of the present invention. DETAILED DESCRIPTION
[0050] In order to make the purpose, technical solution and advantages of the present invention clearer and more specific, the present invention is further described in detail below with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0051] Diamond has attracted everyone's attention due to its extremely excellent physical and chemical properties. However, the reserves of natural diamond are limited, so people have developed a variety of synthetic diamond methods, such as high temperature and high pressure method (HPHT, High pressure High temperature), hot filament chemical vapor deposition method (HFCVD, hot filament chemical vapor deposition), etc. Among them, the microwave plasma chemical vapor deposition method (MPCVD, Microwave plasma chemical vapor deposition) synthetic diamond method can synthesize high-quality and large-area diamonds without the introduction of impurities. It has the advantages of no electrode discharge pollution, fast deposition rate, good stability, etc., and is considered to be the best method for preparing high-quality single-crystal diamonds.
[0052] At present, the mainstream technology route for synthesizing diamonds by chemical vapor deposition is MPCVD (microwave plasma chemical vapor deposition), which is the most mature technology and the most widely used in the market. The advantages of MPCVD technology are: 1. The reaction chamber is larger, which is more suitable for cultivating large-grain diamonds; 2. No electrodes are required during the plasma generation process, and electrode impurities will not be introduced, making it easier to cultivate high-purity diamonds.
[0053] However, the diamond surface (i.e., the upper surface (generally referred to as the growth surface) and the lower surface (generally referred to as the back surface) obtained after the epitaxial growth of the single crystal diamond synthesized by MPCVD is covered with a layer of opaque sp 2Equivalent impurities (i.e. graphite, amorphous carbon, etc.) make it impossible to inspect the growth of diamonds and determine whether they are qualified.
[0054] In view of the above problems, the present invention designs a method for removing impurities from the surface of diamond based on MPCVD equipment. Hydrogen and oxygen plasma are used to remove sp 2 Equivalent impurities have a strong etching effect, so hydrogen and oxygen plasma in MPCVD equipment can be used to etch the diamond surface sp 2 The impurities mainly composed of carbon are removed, thereby achieving the purpose of removing impurities on the surface of diamond and restoring the transparent appearance of diamond.
[0055] The method for removing impurities from the diamond surface based on MPCVD equipment according to a preferred embodiment of the present invention is as follows: Figure 1 As shown, the method for removing impurities from the diamond surface based on MPCVD equipment includes the following steps:
[0056] Step S10: When a first etching instruction is received, a reaction chamber where the diamond to be etched is located is evacuated according to the first etching instruction.
[0057] Specifically, the diamond to be etched is placed on a molybdenum tray with the growth surface facing upward; the molybdenum tray carrying the diamond to be etched is placed on a substrate table of a reaction chamber of an MPCVD device and is sealed; when a first etching instruction sent by a user is received, the MPCVD device is started, and the reaction chamber where the diamond to be etched is located is vacuumed according to the first etching instruction.
[0058] During the epitaxial growth of diamond by MPCVD equipment, carbon atoms are simultaneously deposited on the surface of diamond seed crystals to form sp 3 (Diamond phase) phase of diamond and sp 2 (non-diamond phase) graphite, amorphous carbon. Because hydrogen and oxygen plasmas 2 The carbon atoms in the phase have a stronger etching effect, making the sp 2 The carbon atoms of the phase are removed, sp 3 However, as the thickness of the diamond increases, the surface of the diamond gets closer to the plasma, and changes in temperature, pressure, microwave energy density and other conditions make it easier for carbon atoms to deposit and grow into sp 2 Therefore, after the single crystal epitaxial growth of diamond is completed, the surface of the diamond is covered with a layer of impurities composed of opaque amorphous carbon and graphite.
[0059] Newly grown diamonds need to undergo pickling, cutting, polishing and other processing techniques. The specific processing steps are determined based on the quality inspection results of the diamonds. Impurities such as graphite and amorphous carbon on the surface of diamonds are opaque and directly hinder the use of microscopes to observe and inspect the diamonds. Therefore, these non-diamond phase impurities (i.e. impurities composed of amorphous carbon and graphite) must be removed before diamond quality inspection.
[0060] During the diamond growth process, the side of the diamond facing up and close to the plasma is defined as the growth side, and the side of the diamond facing down and in contact with the molybdenum support is defined as the back side. There are impurities on both the growth side (front side) and the back side (reverse side), and the impurities on the growth side are more than those on the back side. The surface of the newly grown diamond is black. After etching, the diamond is transparent (except for the polycrystalline at the edge).
[0061] Carbon atoms have sp 2 (non-diamond phase) and sp 3 (Diamond phase) There are two types of hybridization. Among them, the hybridization involving one ns orbital and two np orbitals in the same atom is called sp 2 Hybridization, the three hybrid orbitals formed are called sp 2 Hybrid orbitals. The four hybrid orbitals formed by the hybridization of one ns orbital and three np orbitals in the same atom are called sp 3 Hybrid orbitals. Among all carbon elements, only the carbon atoms in diamond crystals are sp 3 Hybrid orbitals form covalent bonds, so the sp 3 phase can be called diamond phase, relatively, sp 2 The phase can be called a non-diamond phase.
[0062] Hydrogen plasma and oxygen plasma on sp 2 The phase has a strong etching effect, while the sp 3 The etching effect of the sp phase is relatively weak, and oxygen plasma is stronger than hydrogen plasma. Based on this principle, a plasma mixed with hydrogen and oxygen with stronger etching effect can be used to etch the sp 2 The diamond growth surface with more impurities such as graphite and amorphous carbon is etched, and the back of the diamond with less impurities is etched with hydrogen plasma, which has a relatively mild etching effect, to remove the non-diamond (sp 2 Phase carbon atom impurities) The purpose of phase impurities.
[0063] like Figure 2As shown in the figure, in the specific implementation process, the diamond crystal to be tested is first pre-treated, immersed in anhydrous ethanol for ultrasonic cleaning for 5 minutes, and then dried to remove surface impurities, and then the growth surface of the diamond crystal to be tested is placed on the molybdenum tray, and then the molybdenum tray carrying the diamond is placed on the substrate table in the MPCVD reaction chamber, and then the cabin door is closed to seal the reaction chamber. After that, the MPCVD equipment is started and the chamber is evacuated to the background vacuum.
[0064] The specific process of vacuuming is as follows: first open the bypass low-flow vacuum pipeline, and reduce the reaction chamber pressure to the set intermediate target pressure value (generally set to 40~50Torr) at a slower pumping speed, and then open the main pumping pipeline to increase the pumping speed, and finally pump the reaction chamber pressure to the set lower target pressure value (generally set to the reaction chamber background vacuum pressure value).
[0065] Step S20, when the vacuum treatment is completed, hydrogen and oxygen in a preset flow range are filled into the reaction chamber, and the hydrogen and oxygen are subjected to plasma excitation treatment to obtain hydrogen-oxygen plasma, wherein the hydrogen-oxygen plasma includes hydrogen plasma and oxygen plasma.
[0066] Specifically, when the vacuum treatment is completed, hydrogen gas within a first preset flow range is filled into the reaction chamber, and the gas pressure in the reaction chamber is monitored in real time; when the gas pressure in the chamber reaches the first preset pressure range, the hydrogen gas is subjected to plasma excitation treatment to obtain hydrogen plasma, and the growth surface of the diamond to be etched is initially etched according to the hydrogen plasma; the flow rate of the hydrogen gas is increased, and when the flow rate of the hydrogen gas reaches a second preset flow range, oxygen gas within a third preset flow range is filled into the reaction chamber; the gas pressure in the chamber and the microwave power in the chamber are increased, and the surface temperature of the diamond to be etched is monitored in real time; when the surface temperature reaches the first preset temperature range, the oxygen gas is subjected to plasma excitation treatment to obtain oxygen plasma.
[0067] The specific implementation operations on the MPCVD equipment are: click the [Vacuum] button on the equipment screen, the system will automatically vacuum and clean the reaction chamber, after this step is completed, click the [Ignition] button, the system will automatically start the ignition procedure, when the ignition procedure of the reaction chamber is completed, click the [Automatic Temperature Increase] button again, the system will automatically start the temperature and pressure increase procedure until the reaction reaches the preset microwave power and gas pressure values.
[0068] The specific operation steps of [Ignition] are as follows: [Ignition] option is used to set the parameters of the system automatic ignition control process. Click [Initial Air Pressure (Torr)] button to set the system initial ignition air pressure; click [H 2Flow Increase (SCCM / sec)] button to set the H 2 Flow rate; click [Open microwave 2 Flow (SCCM)] button to set the H 2 Maximum flow; click [H 2 Maximum flow (SCCM)] button to set the H 2 Click the [Air Pressure (Torr)] button to set the target air pressure value for the reaction chamber ignition; click the [Power (W)] button to set the initial power value for the reaction chamber ignition; click the [Reflected Power Limit (W)] button to set the maximum reflected power during the ignition process; click the [Target Air Pressure (Torr)] button to set the target air pressure value when the ignition process is completed; check the [Temperature Rise] button, and the system will automatically enter the temperature rise step after ignition is completed.
[0069] like Figure 2 As shown, after hydrogen is introduced into the MPCVD equipment, it is necessary to control the hydrogen flow rate to 50-100 sccm (i.e., the first preset flow rate range in the present invention, and the data range preferably adopted in the present invention is obtained by the present invention based on experimental tests), and the gas pressure in the reaction chamber is 5-10 Torr (i.e., the first preset gas pressure range in the present invention). After the gas pressure stabilizes, the microwave power supply is started, and the plasma is ignited to excite the plasma (hydrogen is filled here, and hydrogen plasma is generated after ignition. When hydrogen plasma is generated, the growth surface of the diamond to be detected will be etched first, which is the initial etching treatment in the present invention).
[0070] Further, the hydrogen flow rate is increased to 200-300 sccm (i.e., the second preset flow rate range in the present invention), and oxygen is introduced at a flow rate of 1-2 sccm (i.e., the third preset flow rate range in the present invention), and then the microwave power and the gas pressure in the reaction chamber are increased to make the diamond surface temperature reach 800-900°C (i.e., the first preset temperature range in the present invention) and then keep the temperature stable. At this time, oxygen is input into the reaction chamber of the MPCVD equipment for plasma excitation treatment to generate oxygen plasma.
[0071] Step S30, performing growth surface etching treatment on the growth surface of the diamond to be etched according to the hydrogen-oxygen plasma to complete the removal of impurities from the growth surface of the diamond to be etched.
[0072] Specifically, the growth surface of the diamond to be etched is etched according to the hydrogen plasma and the oxygen plasma. When the time of the growth surface etching reaches a first preset time range, the MPCVD device is turned off to cool the cavity. When the surface temperature of the diamond after cavity cooling is consistent with the room temperature, the cooled diamond is taken out from the reaction chamber of the MPCVD device, and the etching of the growth surface of the diamond to be etched is completed.
[0073] When the hydrogen and oxygen plasma are generated, the hydrogen and oxygen plasma is allowed to etch the diamond growth surface for 120 to 240 minutes (i.e., the first preset time range in the present invention). The general principle of the hydrogen and oxygen plasma etching reaction is as follows: when hydrogen atoms etch, first a free hydrogen atom adsorbs onto the graphite surface and forms a bond with the carbon atom on the surface, and then another hydrogen atom adsorbs onto the same carbon atom to form a dihydride, while the C-C bond breaks, and the graphite structure is gradually destroyed by etching. When oxygen atoms etch, free oxygen atoms adsorb onto the graphite surface and form a bond with the carbon atom on the surface, while the C-C bond breaks, and the graphite structure is destroyed by etching. Figure 2 As shown, when etching is completed, the MPCVD equipment is turned off, and after waiting for a few minutes, the molybdenum support and diamond are taken out and cooled to room temperature.
[0074] The surface of the etched diamond is transparent, but during the etching process, due to the influence of high temperature and brightness in the reaction chamber, it is not possible to accurately judge whether it is completely etched through the observation window. Therefore, to accurately judge whether it is completely etched, you can only wait until the MPCVD machine is shut down and take out the diamond for observation.
[0075] Step S40, when the growth surface etching process is completed and a second etching instruction is received, hydrogen plasma is obtained according to the second etching instruction, and a back side etching process is performed on the back side of the diamond to be etched according to the hydrogen plasma to complete the removal of impurities on the back side of the diamond to be etched.
[0076] Specifically, when the growth surface of the diamond to be etched is etched, the diamond to be etched is placed on the molybdenum tray with the back side facing upward; the molybdenum tray carrying the diamond to be etched is placed on the substrate table and sealed; when the user's second etching instruction is received, the MPCVD equipment is started, and the reaction chamber of the MPCVD equipment is vacuumed; when the vacuuming is completed, hydrogen within the first preset flow range is filled into the reaction chamber, and the gas pressure in the reaction chamber is monitored in real time; when the gas pressure in the chamber is within the first preset pressure range, the hydrogen is plasma-excited to obtain hydrogen plasma.
[0077] The flow rate of the hydrogen gas is increased, and when the flow rate of the hydrogen gas reaches a fourth preset flow rate range, the gas pressure in the cavity and the microwave power in the cavity are increased, and the surface temperature of the diamond to be etched is monitored in real time; when the surface temperature reaches a second preset temperature range, the back side of the diamond to be etched is etched according to the hydrogen plasma, and when the back side etching reaches a second preset time range, the MPCVD device is turned off to cool the cavity; when the surface temperature of the diamond after cavity cooling is consistent with room temperature, the cooled diamond is taken out from the reaction cavity of the MPCVD device, and the back side etching of the diamond to be etched is completed.
[0078] like Figure 3 As shown, the process of removing impurities on the back of diamond by hydrogen plasma etching in the present invention is as follows: 1. Place the diamond crystal on a molybdenum tray with the back facing upward, and place the molybdenum tray carrying the diamond on the substrate table in the MPCVD reaction chamber, close the door, and seal the reaction chamber. 2. Start the MPCVD equipment, evacuate the chamber to the background vacuum, and introduce hydrogen, control the hydrogen flow rate to 50~100sccm, and the pressure in the reaction chamber to 5~10Torr. After the pressure stabilizes, start the microwave power supply to ignite and excite the plasma. 3. Increase the hydrogen flow rate to 300-500sccm (i.e., the first preset flow rate range in the present invention), increase the microwave power and the gas pressure in the reaction chamber, make the temperature of the back of the diamond reach 700-800°C (i.e., the second preset temperature range in the present invention), and then keep the temperature stable, and let the hydrogen plasma etch the back of the diamond for 30-60 minutes (i.e., the second preset time range in the present invention. There are more impurities on the front side, so the hydrogen-oxygen plasma with a stronger etching effect is used for etching, and the etching also takes a relatively longer time, while the back side with fewer impurities only needs to be etched with hydrogen plasma, and the time is relatively shorter). 4. Turn off the MPCVD equipment, wait for a few minutes, and then take out the molybdenum tray and diamond that have cooled to room temperature (observe that the surface of the diamond is transparent to indicate that it has been etched clean).
[0079] Furthermore, after the etching is completed, a quality inspection is required, that is, the surface transparency of the diamond is observed under a microscope to judge the growth quality of the diamond. If the quality inspection result determines that the first etching is not clean, the etching process can be performed again.
[0080] In summary, the present invention is based on the hydrogen and oxygen plasma on sp 2 The principle of stronger etching effect of phase carbon is to use hydrogen and oxygen plasma generated by MPCVD equipment to etch and remove non-diamond (sp 2 Phase impurities (carbon atom impurities) can make the diamond surface clean and transparent, so that it can be observed and inspected under a microscope.
[0081] Furthermore, if Figure 4 As shown, based on the above-mentioned diamond surface impurity removal method based on MPCVD equipment, the present invention also provides a diamond surface impurity removal system based on MPCVD equipment, wherein the diamond surface impurity removal system based on MPCVD equipment includes:
[0082] A vacuum processing module 51 is used for, when receiving a first etching instruction, performing a vacuum processing on the reaction chamber where the diamond to be etched is located according to the first etching instruction;
[0083] The plasma excitation module 52 is used to fill the reaction chamber with hydrogen and oxygen in a preset flow range when the vacuum treatment is completed, and perform plasma excitation treatment on the hydrogen and oxygen to obtain hydrogen-oxygen plasma;
[0084] A growth surface impurity removal module 53 is used to perform growth surface etching treatment on the growth surface of the diamond to be etched according to the hydrogen-oxygen plasma to complete the removal of impurities from the growth surface of the diamond to be etched;
[0085] The back impurity removal module 54, when the growth surface etching process is completed and the second etching instruction is received, obtains hydrogen plasma according to the second etching instruction, and performs back etching process on the back side of the diamond to be etched according to the hydrogen plasma to complete the back impurity removal of the diamond to be etched.
[0086] Furthermore, if Figure 5 As shown, based on the above-mentioned diamond surface impurity removal method and system based on MPCVD equipment, the present invention also provides a terminal accordingly, and the terminal includes a processor 10, a memory 20 and a display 30. Figure 5 Only some components of the terminal are shown, but it should be understood that it is not required to implement all of the components shown, and more or fewer components may be implemented instead.
[0087] In some embodiments, the memory 20 may be an internal storage unit of the terminal, such as a hard disk or memory of the terminal. In other embodiments, the memory 20 may also be an external storage device of the terminal, such as a plug-in hard disk, a smart media card (SMC), a secure digital (SD) card, a flash card, etc. equipped on the terminal. Further, the memory 20 may also include both an internal storage unit of the terminal and an external storage device. The memory 20 is used to store application software and various types of data installed on the terminal, such as the program code of the installation terminal. The memory 20 may also be used to temporarily store data that has been output or is to be output. In one embodiment, a diamond surface impurity removal program 40 based on an MPCVD device is stored on the memory 20, and the diamond surface impurity removal program 40 based on an MPCVD device can be executed by the processor 10, thereby realizing the diamond surface impurity removal method based on an MPCVD device in the present application.
[0088] In some embodiments, the processor 10 may be a central processing unit (CPU), a microprocessor or other data processing chip, used to run the program code or process data stored in the memory 20, such as executing the diamond surface impurity removal method based on the MPCVD device.
[0089] In some embodiments, the display 30 may be an LED display, a liquid crystal display, a touch-sensitive liquid crystal display, an OLED (Organic Light-Emitting Diode) touch device, etc. The display 30 is used to display information on the terminal and to display a visual user interface. The components 10-30 of the terminal communicate with each other via a system bus.
[0090] In one embodiment, when the processor 10 executes the diamond surface impurity removal program 40 based on the MPCVD device in the memory 20, the following steps are implemented:
[0091] When the first etching instruction is received, the reaction chamber where the diamond to be etched is located is vacuumed according to the first etching instruction;
[0092] When the vacuum treatment is completed, hydrogen and oxygen in a preset flow range are filled into the reaction chamber, and the hydrogen and oxygen are subjected to plasma excitation treatment to obtain hydrogen-oxygen plasma;
[0093] Performing a growth surface etching process on the growth surface of the diamond to be etched according to the hydrogen-oxygen plasma to complete the removal of impurities from the growth surface of the diamond to be etched;
[0094] When the growth surface etching process is completed and a second etching instruction is received, hydrogen plasma is obtained according to the second etching instruction, and a back side etching process is performed on the back side of the diamond to be etched according to the hydrogen plasma to complete the removal of impurities on the back side of the diamond to be etched.
[0095] When the first etching instruction is received, the reaction chamber where the diamond to be etched is located is vacuumed according to the first etching instruction, specifically including:
[0096] Place the diamond to be etched on a molybdenum holder with the growth surface facing upward;
[0097] Placing the molybdenum tray carrying the diamond to be etched on the substrate stage of the reaction chamber of the MPCVD device and performing a sealing process;
[0098] When the first etching instruction sent by the user is received, the MPCVD device is started, and the reaction chamber where the diamond to be etched is located is vacuumed according to the first etching instruction.
[0099] Wherein, the hydrogen-oxygen plasma includes hydrogen plasma and oxygen plasma;
[0100] When the vacuuming process is completed, hydrogen and oxygen in a preset flow range are filled into the reaction chamber, and the hydrogen and oxygen are subjected to plasma excitation process to obtain hydrogen-oxygen plasma, which specifically includes:
[0101] When the vacuuming process is completed, hydrogen gas within a first preset flow rate range is filled into the reaction chamber, and the gas pressure in the reaction chamber is monitored in real time;
[0102] When the pressure in the chamber reaches a first preset pressure range, the hydrogen is subjected to plasma excitation treatment to obtain hydrogen plasma, and the growth surface of the diamond to be etched is initially etched according to the hydrogen plasma;
[0103] The reaction chamber is filled with oxygen within a preset flow range, and the oxygen is subjected to plasma excitation treatment to obtain oxygen plasma.
[0104] The step of charging the reaction chamber with oxygen in a preset flow range and performing plasma excitation treatment on the oxygen to obtain oxygen plasma specifically includes:
[0105] The flow rate of the hydrogen is increased, and when the flow rate of the hydrogen reaches the second preset flow rate range, oxygen within a third preset flow rate range is filled into the reaction chamber;
[0106] Increasing the gas pressure and microwave power in the cavity, and monitoring the surface temperature of the diamond to be etched in real time;
[0107] When the surface temperature reaches a first preset temperature range, the oxygen is subjected to plasma excitation treatment to obtain oxygen plasma.
[0108] The step of performing growth surface etching on the growth surface of the diamond to be etched according to the hydrogen-oxygen plasma to remove impurities from the growth surface of the diamond to be etched specifically includes:
[0109] performing growth surface etching treatment on the growth surface of the diamond to be etched according to the hydrogen plasma and the oxygen plasma, and when the time of the growth surface etching treatment reaches a first preset time range, shutting down the MPCVD device to cool the cavity;
[0110] When the surface temperature of the diamond after the cavity is cooled is consistent with the room temperature, the diamond that has been cooled is taken out from the reaction chamber of the MPCVD equipment, and the growth surface of the diamond to be etched is etched.
[0111] When the growth surface etching process is completed and the second etching instruction is received, obtaining hydrogen plasma according to the second etching instruction specifically includes:
[0112] When the growth surface of the diamond to be etched is completely etched, the diamond to be etched is placed on the molybdenum support with the back side facing upward;
[0113] Placing the molybdenum support carrying the diamond to be etched on the substrate table and performing sealing treatment;
[0114] When receiving the second etching instruction from the user, the MPCVD device is started, and a reaction chamber of the MPCVD device is vacuumed;
[0115] When the vacuuming process is completed, hydrogen gas within the first preset flow rate range is filled into the reaction chamber, and the gas pressure in the reaction chamber is monitored in real time;
[0116] When the gas pressure in the cavity is within the first preset gas pressure range, the hydrogen gas is subjected to plasma excitation processing to obtain hydrogen plasma.
[0117] The step of performing back etching on the back side of the diamond to be etched according to the hydrogen plasma to remove impurities on the back side of the diamond to be etched specifically includes:
[0118] The flow rate of the hydrogen is increased, and when the flow rate of the hydrogen reaches a fourth preset flow rate range, the gas pressure in the cavity and the microwave power in the cavity are increased, and the surface temperature of the diamond to be etched is monitored in real time;
[0119] When the surface temperature reaches a second preset temperature range, a back side etching process is performed on the back side of the diamond to be etched according to the hydrogen plasma, and when the back side etching process reaches a second preset time range, the MPCVD device is turned off to cool the cavity;
[0120] When the surface temperature of the diamond after the cavity is cooled is consistent with the room temperature, the diamond that has been cooled is taken out from the reaction chamber of the MPCVD equipment, and the back etching of the diamond to be etched is completed.
[0121] The present invention also provides a computer-readable storage medium, wherein the computer-readable storage medium stores a diamond surface impurity removal program based on MPCVD equipment, and when the diamond surface impurity removal program based on MPCVD equipment is executed by a processor, the steps of the diamond surface impurity removal method based on MPCVD equipment as described above are implemented.
[0122] In summary, the present invention provides a method for removing impurities from the surface of diamond based on MPCVD equipment and related equipment, the method comprising: when a first etching instruction is received, vacuuming the reaction chamber where the diamond to be etched is located according to the first etching instruction; when the vacuuming treatment is completed, hydrogen and oxygen in a preset flow range are filled into the reaction chamber, and the hydrogen and oxygen are subjected to plasma excitation treatment to obtain hydrogen-oxygen plasma; the growth surface of the diamond to be etched is subjected to growth surface etching treatment according to the hydrogen-oxygen plasma to complete the removal of impurities from the growth surface of the diamond to be etched; when the growth surface etching treatment is completed and a second etching instruction is received, hydrogen plasma is obtained according to the second etching instruction, and the back side of the diamond to be etched is subjected to back side etching treatment according to the hydrogen plasma to complete the removal of impurities from the back side of the diamond to be etched. The present invention generates corresponding hydrogen-oxygen plasma by inputting different contents of hydrogen and oxygen, which can respectively realize the effective removal of impurities on the surface of the diamond after epitaxial growth, so that the diamond can restore its transparent appearance and ensure the smooth progress of the diamond quality inspection process.
[0123] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or terminal including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or terminal. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the presence of other identical elements in the process, method, article or terminal including the element.
[0124] Of course, those skilled in the art can understand that all or part of the processes in the above-mentioned embodiments can be implemented by instructing related hardware (such as a processor, a controller, etc.) through a computer program, and the program can be stored in a computer-readable storage medium that can be read by a computer, and the program can include the processes of the above-mentioned method embodiments when executed. The computer-readable storage medium can be a memory, a disk, an optical disk, etc.
[0125] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A method for removing impurities from diamond surface based on MPCVD equipment, characterized in that: The method for removing impurities from the diamond surface based on MPCVD equipment comprises: When the first etching instruction is received, the reaction chamber where the diamond to be etched is located is vacuumed according to the first etching instruction; During the diamond growth process, the side of the diamond facing upward and close to the plasma is defined as the growth side, and the side of the diamond facing downward and in contact with the molybdenum support is defined as the back side. There are impurities on both the growth side and the back side, with more impurities on the growth side than on the back side. Oxygen plasma is more effective than hydrogen plasma in etching. A plasma mixed with hydrogen and oxygen is used to etch the growth surface of diamond, while hydrogen plasma is used to etch the back surface of diamond. When the first etching instruction is received, the reaction chamber where the diamond to be etched is located is vacuumed according to the first etching instruction, specifically including: Place the diamond to be etched on a molybdenum holder with the growth surface facing upward; Placing the molybdenum tray carrying the diamond to be etched on the substrate stage of the reaction chamber of the MPCVD device and performing a sealing process; When receiving the first etching instruction sent by the user, the MPCVD device is started, and the reaction chamber where the diamond to be etched is located is vacuumed according to the first etching instruction; When the vacuum treatment is completed, hydrogen and oxygen in a preset flow range are filled into the reaction chamber, and the hydrogen and oxygen are subjected to plasma excitation treatment to obtain hydrogen-oxygen plasma; The hydrogen-oxygen plasma includes hydrogen plasma and oxygen plasma; When the vacuuming process is completed, hydrogen and oxygen in a preset flow range are filled into the reaction chamber, and the hydrogen and oxygen are subjected to plasma excitation process to obtain hydrogen-oxygen plasma, which specifically includes: When the vacuuming process is completed, hydrogen gas within a first preset flow rate range is filled into the reaction chamber, and the gas pressure in the reaction chamber is monitored in real time; When the pressure in the chamber reaches a first preset pressure range, the hydrogen is subjected to plasma excitation treatment to obtain hydrogen plasma, and the growth surface of the diamond to be etched is initially etched according to the hydrogen plasma; Filling the reaction chamber with oxygen within a preset flow range, and performing plasma excitation treatment on the oxygen to obtain oxygen plasma; The step of charging the reaction chamber with oxygen in a preset flow range and performing plasma excitation treatment on the oxygen to obtain oxygen plasma specifically includes: The flow rate of the hydrogen is increased, and when the flow rate of the hydrogen reaches the second preset flow rate range, oxygen within a third preset flow rate range is filled into the reaction chamber; Increasing the gas pressure and microwave power in the cavity, and monitoring the surface temperature of the diamond to be etched in real time; When the surface temperature reaches a first preset temperature range, the oxygen is subjected to plasma excitation treatment to obtain oxygen plasma; Performing a growth surface etching process on the growth surface of the diamond to be etched according to the hydrogen-oxygen plasma to complete the removal of impurities from the growth surface of the diamond to be etched; The step of performing growth surface etching treatment on the growth surface of the diamond to be etched according to the hydrogen-oxygen plasma to remove impurities from the growth surface of the diamond to be etched specifically includes: performing growth surface etching treatment on the growth surface of the diamond to be etched according to the hydrogen plasma and the oxygen plasma, and when the time of the growth surface etching treatment reaches a first preset time range, shutting down the MPCVD device to cool the cavity; When the surface temperature of the diamond after the cavity is cooled is consistent with the room temperature, the cooled diamond is taken out from the reaction chamber of the MPCVD device, and the growth surface of the diamond to be etched is etched; When the growth surface etching process is completed and a second etching instruction is received, hydrogen plasma is obtained according to the second etching instruction, and a back side etching process is performed on the back side of the diamond to be etched according to the hydrogen plasma to complete the removal of impurities on the back side of the diamond to be etched.
2. The method for removing impurities from the diamond surface based on MPCVD equipment according to claim 1, characterized in that: When the growth surface etching process is completed and the second etching instruction is received, obtaining hydrogen plasma according to the second etching instruction specifically includes: When the growth surface of the diamond to be etched is completely etched, the diamond to be etched is placed on the molybdenum support with the back side facing upward; Placing the molybdenum support carrying the diamond to be etched on the substrate table and performing sealing treatment; When receiving the second etching instruction from the user, the MPCVD device is started, and a reaction chamber of the MPCVD device is vacuumed; When the vacuuming process is completed, hydrogen gas within the first preset flow rate range is filled into the reaction chamber, and the gas pressure in the reaction chamber is monitored in real time; When the gas pressure in the cavity is within the first preset gas pressure range, the hydrogen gas is subjected to plasma excitation processing to obtain hydrogen plasma.
3. The method for removing impurities from the diamond surface based on MPCVD equipment according to claim 1, characterized in that: The step of performing backside etching on the backside of the diamond to be etched according to the hydrogen plasma to remove impurities on the backside of the diamond to be etched specifically includes: The flow rate of the hydrogen is increased, and when the flow rate of the hydrogen reaches a fourth preset flow rate range, the gas pressure in the cavity and the microwave power in the cavity are increased, and the surface temperature of the diamond to be etched is monitored in real time; When the surface temperature reaches a second preset temperature range, a back side etching process is performed on the back side of the diamond to be etched according to the hydrogen plasma, and when the back side etching process reaches a second preset time range, the MPCVD device is turned off to cool the cavity; When the surface temperature of the diamond after the cavity is cooled is consistent with the room temperature, the diamond that has been cooled is taken out from the reaction chamber of the MPCVD equipment, and the back etching of the diamond to be etched is completed.
4. A diamond surface impurity removal system based on MPCVD equipment, characterized in that: The diamond surface impurity removal system based on MPCVD equipment includes: A vacuum processing module, for performing a vacuum processing on a reaction chamber where the diamond to be etched is located according to the first etching instruction when receiving the first etching instruction; During the diamond growth process, the side of the diamond facing upward and close to the plasma is defined as the growth side, and the side of the diamond facing downward and in contact with the molybdenum support is defined as the back side. There are impurities on both the growth side and the back side, with more impurities on the growth side than on the back side. Oxygen plasma is more effective than hydrogen plasma in etching. A plasma mixed with hydrogen and oxygen is used to etch the growth surface of diamond, while hydrogen plasma is used to etch the back surface of diamond. When the first etching instruction is received, the reaction chamber where the diamond to be etched is located is vacuumed according to the first etching instruction, specifically including: Place the diamond to be etched on a molybdenum holder with the growth surface facing upward; Placing the molybdenum tray carrying the diamond to be etched on the substrate stage of the reaction chamber of the MPCVD device and performing a sealing process; When receiving the first etching instruction sent by the user, the MPCVD device is started, and the reaction chamber where the diamond to be etched is located is vacuumed according to the first etching instruction; A plasma excitation module, used for filling the reaction chamber with hydrogen and oxygen within a preset flow range when the vacuum treatment is completed, and performing plasma excitation treatment on the hydrogen and oxygen to obtain hydrogen-oxygen plasma; The hydrogen-oxygen plasma includes hydrogen plasma and oxygen plasma; When the vacuuming process is completed, hydrogen and oxygen in a preset flow range are filled into the reaction chamber, and the hydrogen and oxygen are subjected to plasma excitation process to obtain hydrogen-oxygen plasma, which specifically includes: When the vacuuming process is completed, hydrogen gas within a first preset flow rate range is filled into the reaction chamber, and the gas pressure in the reaction chamber is monitored in real time; When the pressure in the chamber reaches a first preset pressure range, the hydrogen is subjected to plasma excitation treatment to obtain hydrogen plasma, and the growth surface of the diamond to be etched is initially etched according to the hydrogen plasma; Filling the reaction chamber with oxygen within a preset flow range, and performing plasma excitation treatment on the oxygen to obtain oxygen plasma; The step of charging the reaction chamber with oxygen in a preset flow range and performing plasma excitation treatment on the oxygen to obtain oxygen plasma specifically includes: The flow rate of the hydrogen is increased, and when the flow rate of the hydrogen reaches the second preset flow rate range, oxygen within a third preset flow rate range is filled into the reaction chamber; Increasing the gas pressure and microwave power in the cavity, and monitoring the surface temperature of the diamond to be etched in real time; When the surface temperature reaches a first preset temperature range, the oxygen is subjected to plasma excitation treatment to obtain oxygen plasma; A growth surface impurity removal module, used for performing growth surface etching treatment on the growth surface of the diamond to be etched according to the hydrogen-oxygen plasma to complete the removal of impurities from the growth surface of the diamond to be etched; The step of performing growth surface etching treatment on the growth surface of the diamond to be etched according to the hydrogen-oxygen plasma to remove impurities from the growth surface of the diamond to be etched specifically includes: performing growth surface etching treatment on the growth surface of the diamond to be etched according to the hydrogen plasma and the oxygen plasma, and when the time of the growth surface etching treatment reaches a first preset time range, shutting down the MPCVD device to cool the cavity; When the surface temperature of the diamond after the cavity is cooled is consistent with the room temperature, the cooled diamond is taken out from the reaction chamber of the MPCVD device, and the growth surface of the diamond to be etched is etched; The back impurity removal module obtains hydrogen plasma according to the second etching instruction when the growth surface etching process is completed and the second etching instruction is received, and performs back etching process on the back side of the diamond to be etched according to the hydrogen plasma to complete the back impurity removal of the diamond to be etched.
5. A terminal, characterized in that: The terminal includes: a memory, a processor, and a diamond surface impurity removal program based on MPCVD equipment stored in the memory and executable on the processor. When the diamond surface impurity removal program based on MPCVD equipment is executed by the processor, the steps of the diamond surface impurity removal method based on MPCVD equipment as described in any one of claims 1 to 3 are implemented.
6. A computer-readable storage medium, characterized in that: The computer-readable storage medium stores a diamond surface impurity removal program based on MPCVD equipment, and when the diamond surface impurity removal program based on MPCVD equipment is executed by a processor, the steps of the diamond surface impurity removal method based on MPCVD equipment as described in any one of claims 1-3 are implemented.
Citation Information
Patent Citations
Method for removing silicon carbide on surface of diamond window prepared on silicon substrate by utilizing hydrogen plasma
CN107546109A
High-efficiency treatment method and device for diamond micro-powder
CN111286713A