Preparation method of corncob-derived biomass porous carbon electrode material

The preparation method of porous carbon electrode material derived from corn cob has solved the problem of poor performance of biomass carbon materials, and realized an electrode material with high specific capacity and stability, which is suitable for the positive electrode of aqueous zinc-ion batteries.

CN118579779BActive Publication Date: 2026-11-24NORTHEAST DIANLI UNIVERSITY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410751494.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-12
Publication Date
2026-11-24
Estimated Expiration
2044-06-12

AI Technical Summary

Technical Problem

Existing biochar materials have poor performance as cathode materials for aqueous zinc-ion batteries, and their preparation methods are relatively simple, making it difficult to meet the requirements of practical applications.

Method used

Using corn cobs as a carbon source, biomass porous carbon electrode materials doped with N, O, F, Cl, P and Zn heteroatoms were prepared by hydrothermal pretreatment and eutectic solvent activation. The process included hydrothermal pretreatment, eutectic solvent mixing, carbonization and acid washing, forming a rich mesoporous structure.

Benefits of technology

The specific capacity, rate performance, and cycle stability of the material were improved, enabling the efficient conversion of agricultural and forestry waste and producing high-performance electrode materials suitable for mass production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118579779B_ABST
    Figure CN118579779B_ABST
Patent Text Reader

Abstract

This invention discloses a method for preparing porous carbon electrode materials derived from corn cob biomass, belonging to the field of materials technology. First, the biomass undergoes hydrothermal pretreatment in a mixed solution of HCl and NH4F, followed by activation and carbonization treatment using a ZnCl2-acetamide eutectic solvent. The hydrothermal pretreatment decomposes some of the cellulose and hemicellulose in the corn cob and serves as a pre-carbonization process, which is beneficial for forming a larger specific surface area during the subsequent high-temperature carbonization and activation treatment. The use of a eutectic solvent increases the graphitization degree of the biomass carbon, thereby increasing its specific surface area and porosity. Furthermore, both of these treatments promote heteroatom doping. The biomass carbon prepared by the method of this invention is a multi-heteroatom-doped carbon material containing N, O, F, Cl, P, and Zn, assembled from nanoparticles, possessing a porous structure. Through compositional and structural regulation, the electrochemical performance of the material is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of materials technology, and in particular relates to a method for preparing a porous carbon electrode material derived from corn cob biomass. Background Technology

[0002] In the face of severe energy and environmental challenges, the development of renewable clean energy and energy storage and conversion technologies is imperative. Lithium-ion batteries, favored for their high energy density, long lifespan, and flexible configuration, are widely used in consumer electronics. However, their application in large-scale energy storage is constrained by lithium resource shortages and safety concerns. Developing inexpensive and environmentally friendly new energy storage battery technologies is urgently needed. Among numerous novel secondary energy storage devices, aqueous zinc-ion batteries have a theoretical specific capacity of 829 mAh·g. -1 Zinc-ion batteries can be assembled in air, and the zinc salt used as the electrolyte is inexpensive and readily available. Furthermore, the radius of zinc ions is very close to that of lithium ions. Rechargeable zinc-ion batteries use divalent ions as transport carriers, and their insertion / extraction reactions involve multiple electrons, enabling higher discharge specific capacity and energy density. They are considered one of the economical and ideal electrochemical energy storage devices for new environments. However, the high water activity in aqueous electrolytes can cause problems such as hydrogen evolution and corrosion, and due to the presence of zinc... 2+ The strong electrostatic interaction with the cathode material accelerates the dissolution and collapse of the cathode material, which greatly affects the specific capacity and cycle stability of the battery.

[0003] Cathode materials, as a crucial component of aqueous zinc-ion batteries, are one of the decisive factors affecting their performance. Currently, commonly used cathode materials mainly include manganese-based oxides, vanadium-based oxides, Prussian blue analogs, and organic compounds. Manganese-based materials affected by the Jahn-Teller effect, Prussian blue analogs with insufficient specific capacity, organic materials with complex mechanisms, and vanadium-based materials prone to dissolution and collapse all struggle to meet practical application standards. Biochar materials, on the other hand, are abundant, inexpensive, and possess excellent stability and conductivity. By controlling the pore distribution, carrier migration can be promoted, which is beneficial for improving their electrochemical energy storage performance. Zou et al. prepared biochar electrode materials using corn silk as a biomass carbon source after KOH activation. After assembling them into a zinc-ion hybrid supercapacitor, they achieved a performance of 0.2 A·g⁻¹. -1 The specific capacity at that time was 87mAh·g -1(Zou Z, LuoX, Wang L, et al. Highly mesoporous carbons derived from corn silks as high performance electrode materials of supercapacitors and zinc ion capacitors[J]. Journal of Energy Storage, 2021,44:103385.).

[0004] Existing research has shown that biochar has certain application potential as a cathode material for aqueous zinc ion energy storage devices, but its preparation method is relatively simple, and its specific capacity, rate performance, cycle stability and other properties can still be further improved.

[0005] Therefore, there is an urgent need for a new technical solution to optimize the preparation method of biomass carbon electrode materials and improve their electrochemical performance. Summary of the Invention

[0006] The technical problem to be solved by the present invention is to provide a method for preparing a porous carbon electrode material derived from corn cob, which solves the technical problem that the preparation method of biomass carbon material is relatively simple in the existing new energy storage battery technology, and its performance as a positive electrode material of aqueous zinc-ion battery is poor.

[0007] The technical solution adopted in this invention is to provide a method for preparing a porous carbon electrode material derived from corn cob biomass, comprising the following steps:

[0008] (1) Hydrothermal pretreatment of corn cobs

[0009] ① Wash the collected corn cobs with ultrapure water to remove the dust on the outer surface, soak them in ultrapure water and place them in a constant temperature oven for a certain period of time;

[0010] ② The corn cobs obtained in step ① are freeze-dried;

[0011] ③ Use a high-speed blender to crush the sample obtained in step ②, and sieve the crushed powder through a 65-mesh sieve;

[0012] ④ The corn cob powder obtained in step ③ is soaked in a mixture of NH4F and HCl for hydrothermal pretreatment;

[0013] ⑤ Wash the soaked corn cob powder with ultrapure water and freeze-dry it. The resulting dark brown powder is the pretreated corn cob sample.

[0014] (2) Preparation of porous carbon derived from corn cob biomass

[0015] ① The pretreated corn cob powder obtained in step (1) is mixed with a eutectic solvent formed by ZnCl2-acetamide and activated;

[0016] ② The mixture of ZnCl2-acetamide eutectic solvent and corn cob was transferred into a high-temperature tube furnace and carbonized at high temperature under a nitrogen atmosphere;

[0017] ③ After the furnace temperature drops to room temperature, the activated product is acid-washed to remove excess metal ions, and then the powder is washed with deionized water until the pH is neutral. After freeze-drying, the corn cob-derived biomass porous carbon electrode material is obtained.

[0018] In step (1), the temperature of the constant temperature oven in step ① is 50-100℃, and the soaking time is 12-48h.

[0019] In step (1) ④, the mass of the corn cob is 1–5 g, the amount of NH4F added is 0.1–0.8 mol, and the concentration of HCl is 3–8 mol·L⁻¹. -1 The hydrothermal pretreatment conditions are 60–110℃ for 12–120 h.

[0020] In step (2), ZnCl2 and acetamide are mixed and placed in an oven at 90-110°C for 1-4 hours to form a eutectic solvent.

[0021] In step (2) ①, the mass ratio of corn cob to ZnCl2 is 1:1 to 1:6, the mass ratio of ZnCl2 to acetamide is 3:1.5 to 3:5, the activation temperature is 90 to 120℃, and the activation time is 6 to 24h.

[0022] In step (2) ②, the high-temperature carbonization conditions are 700-900℃ for 2-4 hours.

[0023] The acid washing conditions in step (2) ③ are 4–8 mol·L⁻¹. -1 Soak in H2SO4 for 4–12 hours.

[0024] The porous carbon electrode material of corn cob-derived biomass prepared according to the above method is a carbon material doped with N, O, F, Cl, P and Zn heteroatoms. It is assembled from nanoparticles and has a rich mesoporous structure.

[0025] An electrode that uses the aforementioned corn cob-derived biomass porous carbon as the electrode active material.

[0026] An aqueous zinc-ion battery uses the aforementioned electrodes as the positive electrode.

[0027] Through the above design scheme, the present invention can bring the following beneficial effects:

[0028] (1) This invention selects corn cobs, an agricultural waste, as the carbon source to conduct research on the preparation of porous carbon electrode materials derived from corn cob biomass. This achieves the clean and efficient conversion of agricultural and forestry waste into high-value-added electrode materials, solving the problems of high cost and low specific capacity in the current preparation of carbon-based electrode materials. This invention fully utilizes the unique composition and structural characteristics of corn cobs, optimizes the experimental scheme, and prepares porous carbon electrode materials derived from corn cob biomass. These materials are N, O, F, Cl, P, and Zn multi-heteroatom-doped carbon materials, assembled from nanoparticles, possessing a porous structure and a specific surface area of ​​991.19 m². 2 ·g -1 The average pore volume is 0.68 cm³. 3 ·g -1 The main pore structure is mesoporous. By doping atoms and controlling the pore structure, the electrochemical activity, conductivity, and carrier migration and storage processes of the material are effectively improved, thereby enhancing the material's specific capacity, rate performance, and cycle stability.

[0029] (2) The innovative material synthesis method of this invention first performs hydrothermal pretreatment on biomass, and then uses a eutectic solvent as an activator to activate and carbonize it. Corn cobs are completely immersed in a mixed solution of HCl and NH4F and undergo a relatively long hydrothermal pretreatment process at a certain temperature. The corn cobs decompose some of the cellulose and hemicellulose through acid hydrolysis. At the same time, this hydrothermal process can still serve the purpose of pre-carbonization, which is beneficial to forming a larger specific surface area in the subsequent high-temperature carbonization and activation process. After this hydrothermal pretreatment, heteroatoms such as N, F, and Cl can be further doped into the carbon material, thereby improving the electrochemical activity and surface wettability of the material. Furthermore, the hydrothermal pretreated corn cobs are mixed with a eutectic solvent formed by ZnCl2-acetamide. On the one hand, the eutectic solvent can be fully mixed with biomass, which is beneficial for high-temperature carbonization activation treatment. On the other hand, during the eutectic solvent-assisted activation and high-temperature carbonization process, ZnCl2 can be used as a dehydrating agent and carbonization activator to improve the graphitization degree of biochar. Acetamide generates gaseous substances during the carbonization process, which is beneficial for increasing the specific surface area and porosity of biochar, and can also promote heteroatom doping.

[0030] (3) The preparation method provided by this invention is scientific, reasonable, safe, easy to implement, requires simple equipment, has low cost, and is highly controllable. It is suitable for the mass production of porous carbon electrode materials derived from corn cob biomass. At the same time, this method can also be extended to the controllable and large-scale preparation of other multi-heteroatom doped biomass carbon electrode materials. Attached Figure Description

[0031] Figure 1This is a SEM image of the biomass porous carbon electrode material prepared in Example 2 of the preparation method of a corn cob-derived biomass porous carbon electrode material of the present invention;

[0032] Figure 2 This is a TEM image of the biomass porous carbon electrode material prepared in Example 2 of the preparation method of a corn cob-derived biomass porous carbon electrode material of the present invention;

[0033] Figure 3 This is an EDS elemental distribution diagram of the biomass porous carbon electrode material prepared in Example 2 of the preparation method of a corn cob-derived biomass porous carbon electrode material of the present invention;

[0034] Figure 4 The image shows the XRD pattern of the biomass porous carbon electrode material prepared in Example 2 of the preparation method of a corn cob-derived biomass porous carbon electrode material of the present invention.

[0035] Figure 5 The Raman test results are for the biomass porous carbon electrode material prepared in Example 2 of the preparation method of a corn cob-derived biomass porous carbon electrode material of the present invention.

[0036] Figure 6 The N2 adsorption / desorption isotherm and pore size distribution diagram of the biomass porous carbon electrode material prepared in Example 2 of the preparation method of corn cob-derived biomass porous carbon electrode material of the present invention are shown.

[0037] Figure 7 The biomass porous carbon electrode material prepared in Example 2 of the preparation method of corn cob-derived biomass porous carbon electrode material of the present invention has a performance of 1-5 mV·s. -1 Cyclic voltammogram at scan rate;

[0038] Figure 8 The biomass porous carbon electrode material prepared in Example 2 of the preparation method of a corn cob-derived biomass porous carbon electrode material of the present invention has a content of 0.1-5 A·g. -1 Constant current charge-discharge diagram at current density. Detailed Implementation

[0039] The present invention will be further described below with reference to the accompanying drawings and specific embodiments:

[0040] Example 1: This example describes a method for preparing a porous carbon electrode material derived from corn cob biomass. The specific steps are as follows:

[0041] 1) Hydrothermal pretreatment of corn cobs

[0042] (1) Wash the collected corn cobs with ultrapure water to remove the dust on the outer surface, soak them in ultrapure water and place them in a constant temperature oven at 100℃ for 12 hours;

[0043] (2) Freeze-dry the corn cobs obtained in step (1);

[0044] (3) Use a wall-breaking machine to crush the sample obtained in step (2), and sieve the crushed powder through a 65-mesh sieve;

[0045] (4) The corn cob powder obtained in step (3) is soaked in a mixture of NH4F and HCl for hydrothermal pretreatment, wherein the mass of the corn cob is 5g, the amount of NH4F added is 0.1mol, and the concentration of HCl is 3mol·L⁻¹. -1 The volume of HCl was 50 mL, the hydrothermal pretreatment temperature was 110℃, and the time was 12 h.

[0046] (5) Wash the corn cob powder obtained in step (4) with ultrapure water until the pH is neutral, and then freeze dry. The resulting dark brown powder is the corn cob sample after hydrothermal pretreatment.

[0047] 2) Preparation of porous carbon derived from corn cob biomass

[0048] (1) After mixing ZnCl2 and acetamide, place them in an oven at 110℃ for 1h to form a eutectic solvent. Mix the hydrothermally pretreated corn cob obtained in step 1) with the ZnCl2-acetamide eutectic solvent and place them in an oven at 90℃ for 24h. The mass of the corn cob is 1g, the mass of ZnCl2 is 1g, and the mass of acetamide is 1.7g.

[0049] (2) The mixture of ZnCl2-acetamide eutectic solvent and corn cob was transferred into a high-temperature tube furnace and kept at 900℃ for 2 hours under a nitrogen atmosphere;

[0050] (3) After the furnace temperature drops to room temperature, the product is treated with 8 mol·L⁻¹ -1 The sample was soaked in H2SO4 solution for 4 hours, then washed with ultrapure water until the pH was neutral, and then freeze-dried to obtain corn cob-derived biomass porous carbon material.

[0051] Example 2: This example describes a method for preparing a porous carbon electrode material derived from corn cob biomass. The specific steps are as follows:

[0052] 1) Hydrothermal pretreatment of corn cobs

[0053] (1) Wash the collected corn cobs with ultrapure water to remove the dust on the outer surface, soak them in ultrapure water and place them in a constant temperature oven at 90℃ for 24 hours;

[0054] (2) Freeze-dry the corn cobs obtained in step (1);

[0055] (3) Use a wall-breaking machine to crush the sample obtained in step (2), and sieve the crushed powder through a 65-mesh sieve;

[0056] (4) The corn cob powder obtained in step (3) is soaked in a mixture of NH4F and HCl for hydrothermal pretreatment, wherein the mass of the corn cob is 3g, the amount of NH4F added is 0.2mol, and the concentration of HCl is 6mol·L⁻¹. -1 The volume of HCl was 50 mL, the hydrothermal pretreatment temperature was 90 °C, and the time was 72 h.

[0057] (5) Wash the corn cob powder obtained in step (4) with ultrapure water until the pH is neutral, and then freeze dry. The resulting dark brown powder is the corn cob sample after hydrothermal pretreatment.

[0058] 2) Preparation of porous carbon derived from corn cob biomass

[0059] (1) After mixing ZnCl2 and acetamide, place them in an oven at 100℃ for 2 hours to form a eutectic solvent. Mix the hydrothermally pretreated corn cob obtained in step 1) with the ZnCl2-acetamide eutectic solvent and place them in an oven at 100℃ for 10 hours. The mass of the corn cob is 1g, the mass of ZnCl2 is 3g, and the mass of acetamide is 2g.

[0060] (2) The mixture of ZnCl2-acetamide eutectic solvent and corn cob was transferred into a high-temperature tube furnace and kept at 850°C for 3 hours under a nitrogen atmosphere;

[0061] (3) After the furnace temperature drops to room temperature, the product is treated with 6 mol·L⁻¹ -1 The sample was soaked in H2SO4 solution for 6 hours, then washed with ultrapure water until the pH was neutral, and then freeze-dried to obtain corn cob-derived biomass porous carbon material.

[0062] Example 3: This example describes a method for preparing a porous carbon electrode material derived from corn cob biomass. The specific steps are as follows:

[0063] 1) Hydrothermal pretreatment of corn cobs

[0064] (1) Wash the collected corn cobs with ultrapure water to remove the dust on the outer surface, soak them in ultrapure water and place them in a constant temperature oven at 80℃ for 32 hours;

[0065] (2) Freeze-dry the corn cobs obtained in step (1);

[0066] (3) Use a wall-breaking machine to crush the sample obtained in step (2), and sieve the crushed powder through a 65-mesh sieve;

[0067] (4) The corn cob powder obtained in step (3) is soaked in a mixture of NH4F and HCl for hydrothermal pretreatment, wherein the mass of the corn cob is 4 g, the amount of NH4F added is 0.8 mol, and the concentration of HCl is 4 mol·L⁻¹. -1 The volume of HCl was 50 mL, the hydrothermal pretreatment temperature was 90 °C, and the time was 48 h.

[0068] (5) Wash the corn cob powder obtained in step (4) with ultrapure water until the pH is neutral, and then freeze dry. The resulting dark brown powder is the corn cob sample after hydrothermal pretreatment.

[0069] 2) Preparation of porous carbon derived from corn cob biomass

[0070] (1) After mixing ZnCl2 and acetamide, place them in an oven at 100℃ for 2 hours to form a eutectic solvent. Mix the hydrothermally pretreated corn cob obtained in step 1) with the ZnCl2-acetamide eutectic solvent and place them in an oven at 100℃ for 20 hours. The mass of the corn cob is 1g, the mass of ZnCl2 is 2g, and the mass of acetamide is 2.4g.

[0071] (2) The mixture of ZnCl2-acetamide eutectic solvent and corn cob was transferred into a high-temperature tube furnace and kept at 850°C for 4 hours under a nitrogen atmosphere;

[0072] (3) After the furnace temperature drops to room temperature, the product is treated with 6 mol·L⁻¹ -1 The sample was soaked in H2SO4 solution for 10 hours, then washed with ultrapure water until the pH was neutral, and then freeze-dried to obtain corn cob-derived biomass porous carbon material.

[0073] Example 4: This example describes a method for preparing a porous carbon electrode material derived from corn cob biomass. The specific steps are as follows:

[0074] 1) Hydrothermal pretreatment of corn cobs

[0075] (1) Wash the collected corn cobs with ultrapure water to remove the dust on the outer surface, soak them in ultrapure water and place them in a constant temperature oven at 70°C for 36 hours;

[0076] (2) Freeze-dry the corn cobs obtained in step (1);

[0077] (3) Use a wall-breaking machine to crush the sample obtained in step (2), and sieve the crushed powder through a 65-mesh sieve;

[0078] (4) The corn cob powder obtained in step (3) is soaked in a mixture of NH4F and HCl for hydrothermal pretreatment, wherein the mass of the corn cob is 3g, the amount of NH4F added is 0.6mol, and the concentration of HCl is 6mol·L.-1 The volume of HCl was 50 mL, the hydrothermal pretreatment temperature was 80 °C, and the time was 72 h.

[0079] (5) Wash the corn cob powder obtained in step (4) with ultrapure water until the pH is neutral, and then freeze dry. The resulting dark brown powder is the corn cob sample after hydrothermal pretreatment.

[0080] 2) Preparation of porous carbon derived from corn cob biomass

[0081] (1) After mixing ZnCl2 and acetamide, place them in an oven at 100℃ for 2 hours to form a eutectic solvent. Mix the hydrothermally pretreated corn cob obtained in step 1) with the ZnCl2-acetamide eutectic solvent and place them in an oven at 100℃ for 16 hours. The mass of the corn cob is 1g, the mass of ZnCl2 is 4g, and the mass of acetamide is 3.2g.

[0082] (2) The mixture of ZnCl2-acetamide eutectic solvent and corn cob was transferred into a high-temperature tube furnace and kept at 800℃ for 3 hours under a nitrogen atmosphere;

[0083] (3) After the furnace temperature drops to room temperature, the product is treated with 6 mol·L⁻¹ -1 The sample was soaked in H2SO4 solution for 8 hours, then washed with ultrapure water until the pH was neutral, and then freeze-dried to obtain corn cob-derived biomass porous carbon material.

[0084] Example 5: This example describes a method for preparing a porous carbon electrode material derived from corn cob biomass. The specific steps are as follows:

[0085] 1) Hydrothermal pretreatment of corn cobs

[0086] (1) The collected corn cobs were washed with ultrapure water to remove the dust on the outer surface, soaked in ultrapure water and placed in a constant temperature oven at 60°C for 48 hours.

[0087] (2) Freeze-dry the corn cobs obtained in step (1);

[0088] (3) Use a wall-breaking machine to crush the sample obtained in step (2), and sieve the crushed powder through a 65-mesh sieve;

[0089] (4) The corn cob powder obtained in step (3) is soaked in a mixture of NH4F and HCl for hydrothermal pretreatment, wherein the mass of the corn cob is 2g, the amount of NH4F added is 0.4mol, and the concentration of HCl is 6mol·L. -1 The volume of HCl was 50 mL, the hydrothermal pretreatment temperature was 70 °C, and the time was 96 h.

[0090] (5) Wash the corn cob powder obtained in step (4) with ultrapure water until the pH is neutral, and then freeze dry. The resulting dark brown powder is the corn cob sample after hydrothermal pretreatment.

[0091] 2) Preparation of porous carbon derived from corn cob biomass

[0092] (1) After mixing ZnCl2 and acetamide, place them in an oven at 100℃ for 2 hours to form a eutectic solvent. Mix the hydrothermally pretreated corn cob obtained in step 1) with the ZnCl2-acetamide eutectic solvent and place them in an oven at 110℃ for 12 hours. The mass of the corn cob is 1g, the mass of ZnCl2 is 6g, and the mass of acetamide is 3g.

[0093] (2) The mixture of ZnCl2-acetamide eutectic solvent and corn cob was transferred into a high-temperature tube furnace and kept at 750°C for 3 hours under a nitrogen atmosphere;

[0094] (3) After the furnace temperature drops to room temperature, the product is treated with 4 mol·L⁻¹ -1 The sample was soaked in H2SO4 solution for 12 hours, then washed with ultrapure water until the pH was neutral, and then freeze-dried to obtain corn cob-derived biomass porous carbon material.

[0095] Example 6: This example describes a method for preparing a porous carbon electrode material derived from corn cob biomass. The specific steps are as follows:

[0096] 1) Hydrothermal pretreatment of corn cobs

[0097] (1) Wash the collected corn cobs with ultrapure water to remove the dust on the outer surface, soak them in ultrapure water and place them in a constant temperature oven at 50°C for 48 hours;

[0098] (2) Freeze-dry the corn cobs obtained in step (1);

[0099] (3) Use a wall-breaking machine to crush the sample obtained in step (2), and sieve the crushed powder through a 65-mesh sieve;

[0100] (4) The corn cob powder obtained in step (3) is soaked in a mixture of NH4F and HCl for hydrothermal pretreatment, wherein the mass of the corn cob is 1g, the amount of NH4F added is 0.2mol, and the concentration of HCl is 8mol·L⁻¹. -1 The volume of HCl was 50 mL, the hydrothermal pretreatment temperature was 60 °C, and the time was 120 h.

[0101] (5) Wash the corn cob powder obtained in step (4) with ultrapure water until the pH is neutral, and then freeze dry. The resulting dark brown powder is the corn cob sample after hydrothermal pretreatment.

[0102] 2) Preparation of porous carbon derived from corn cob biomass

[0103] (1) After mixing ZnCl2 and acetamide, place them in an oven at 90℃ for 4 hours to form a eutectic solvent. Mix the hydrothermally pretreated corn cob obtained in step 1) with the ZnCl2-acetamide eutectic solvent and place it in an oven at 120℃ for 6 hours. The mass of the corn cob is 1g, the mass of ZnCl2 is 5g, and the mass of acetamide is 7.5g.

[0104] (2) The mixture of ZnCl2-acetamide eutectic solvent and corn cob was transferred into a high-temperature tube furnace and kept at 700℃ for 4 hours under a nitrogen atmosphere;

[0105] (3) After the furnace temperature drops to room temperature, the product is treated with 6 mol·L⁻¹ -1 The sample was soaked in H2SO4 solution for 6 hours, then washed with ultrapure water until the pH was neutral, and then freeze-dried to obtain corn cob-derived biomass porous carbon material.

[0106] See Figure 1 As shown in the figure, the corn cob-derived biomass porous carbon electrode material prepared in Example 2 of the present invention was characterized by scanning electron microscopy (SEM). As can be seen from the figure, the biomass carbon material is composed of a large number of nanoparticles, forming a rich pore structure.

[0107] See Figure 2 As shown in the figure, the corn cob-derived biomass porous carbon electrode material prepared in Example 2 of the present invention was characterized by transmission electron microscopy (TEM). As can be seen from the figure, the biomass carbon material has a large number of mesoporous structures and is assembled from nanoparticles, which is consistent with the SEM analysis results.

[0108] See Figure 3 As shown in the figure, the corn cob-derived biomass porous carbon electrode material prepared in Example 2 of the present invention was characterized by EDS elemental distribution. As can be seen from the figure, the biomass carbon material is mainly composed of C, N, O, F, Cl, P and Zn elements, indicating that the material is a carbon material doped with multiple heteroatoms.

[0109] See Figure 4 As shown in the figure, the corn cob-derived biomass porous carbon electrode material prepared in Example 2 of the present invention was characterized by X-ray diffraction (XRD). As can be seen from the figure, the biomass carbon material has two obvious diffraction peaks at 2θ = 25.8° and 42.3°, which correspond to the (002) and (100) crystal planes of the carbon material, respectively.

[0110] See Figure 5 As shown in the figure, the porous carbon electrode material derived from corn cob biomass prepared in Example 2 of this invention was characterized by Raman spectroscopy. The figure shows that the Raman spectrum at 1338 cm⁻¹ is... -1The characteristic peak at that location represents graphite or disordered sp. 2 The defect sites of hybrid carbon atoms are D-bands; at 1586 cm⁻¹ -1 The characteristic peak at that location corresponds to the in-plane vibration of E2g graphitic carbon atoms, which is the G band. Calculations show that... D / I G A value of 1.19 indicates that the biochar material has certain structural defects, with carbon atoms mainly in sp... 2 Hybrid forms exist.

[0111] See Figure 6 As shown, the N2 adsorption / desorption test was performed on the corn cob-derived biomass porous carbon electrode material prepared in Example 2 of this invention, and its specific surface area was 991.19 m². 2 ·g -1 The pore volume is 0.68 cm³. 3 ·g -1 The N2 adsorption / desorption isotherm is a typical Type IV isotherm, indicating that its main pore structure is mesoporous, which is consistent with the results of the pore size distribution diagram.

[0112] See Figure 7 As shown, the porous carbon electrode material derived from corn cob prepared in Example 2 of this invention exhibits performance at 1–5 mV·s. -1 Cyclic voltammetry was performed at a scan rate using Zn foil as the anode, corn cob-derived biomass porous carbon electrode material as the cathode, and a mixed solution of 2M ZnSO4 and 0.2M MnSO4 as the electrolyte. The results showed that the CV curve exhibited an oxidation peak at 1.68 V and significant reduction peaks at 1.17 and 1.32 V. This is due to the oxidation peaks at 1.68 V and 1.17 and 1.32 V, respectively. 2+ and H + This is caused by insertion / extraction within the electrode; furthermore, when the scan rate increases from 1 mV·s... -1 Gradually rise to 5mV·s -1 When the integral area of ​​the cyclic voltammetry curve increases, the shape of the curve remains almost unchanged, indicating that the electrode material has excellent electrochemical reversibility.

[0113] See Figure 8 As shown, the porous carbon electrode material derived from corn cob prepared in Example 2 of this invention is subjected to a temperature range of 0.1–5 A·g. -1 Constant current charge-discharge tests were conducted at different current densities. The test results show that the GCD curves exhibit two discharge plateaus at different current densities, which can be attributed to Zn. 2+ and H + The continuous insertion, and the inflection point at 1.3V, is due to the difference in ion diffusion coefficients between the two; when the current density is 0.1A·g -1 At that time, its discharge specific capacity was 61.6 mAh·g. -1The current density was increased to 5 A·g -1 It can still maintain 48.8% of its initial specific capacity, indicating that it has excellent specific capacity and rate performance.

[0114] The implementation of the present invention is not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and are included within the protection scope of the present invention.

Claims

1. A method for preparing a porous carbon electrode material derived from corn cob biomass, characterized in that: Includes the following steps: (1) Hydrothermal pretreatment of corn cobs The collected corn cobs were washed with ultrapure water to remove the dust on the outer surface, soaked in ultrapure water and placed in a constant temperature oven for a certain period of time. Steps The obtained corn cobs were freeze-dried; Use a high-speed blender to complete the steps. The obtained sample was crushed, and the pulverized powder was sieved through a 65-mesh sieve. Steps The obtained corn cob powder was soaked in a mixture of NH4F and HCl for hydrothermal pretreatment; The corn cob powder was washed with ultrapure water and then freeze-dried to obtain a dark brown powder, which was the pretreated corn cob sample. (2) Preparation of porous carbon derived from corn cob biomass The pretreated corn cob powder obtained in step (1) is mixed with a eutectic solvent formed by ZnCl2-acetamide and activated; the eutectic solvent is formed by mixing ZnCl2 and acetamide and placing them in an oven at 90-110 ℃ for 1-4 h. The mixture of ZnCl2-acetamide eutectic solvent and corn cob was transferred into a high-temperature tube furnace and carbonized at high temperature under a nitrogen atmosphere. After the furnace temperature drops to room temperature, the activated product is acid-washed to remove excess metal ions, and then the powder is washed with deionized water until the pH is neutral. Finally, it is freeze-dried to obtain the corn cob-derived biomass porous carbon electrode material.

2. The method for preparing a porous carbon electrode material derived from corn cob biomass according to claim 1, characterized in that: The step (1) The temperature of the medium constant temperature oven is 50 ~ 100 ℃, and the soaking time is 12 ~ 48 h.

3. The method for preparing a porous carbon electrode material derived from corn cob biomass according to claim 1, characterized in that: The step (1) The mass of the corn cob is 1-5 g, the amount of NH4F added is 0.1-0.8 mol, and the concentration of HCl is 3-8 mol·L⁻¹. -1 The hydrothermal pretreatment conditions are 60 ~ 110 ℃ for 12 ~ 120 h.

4. The method for preparing a porous carbon electrode material derived from corn cob biomass according to claim 1, characterized in that: The step (2) The mass ratio of corn cob to ZnCl2 was 1:1 to 1:6, the mass ratio of ZnCl2 to acetamide was 3:1.5 to 3:5, the activation temperature was 90 to 120 ℃, and the activation time was 6 to 24 h.

5. The method for preparing a porous carbon electrode material derived from corn cob biomass according to claim 1, characterized in that: The step (2) The conditions for medium- and high-temperature carbonization are 700 ~ 900 ℃ for 2 ~ 4 h.

6. The method for preparing a porous carbon electrode material derived from corn cob biomass according to claim 1, characterized in that: The step (2) The acid washing conditions are 4 ~ 8 mol·L⁻¹ -1 Soak in H2SO4 for 4 to 12 hours.

7. The corn cob-derived biomass porous carbon electrode material prepared by the method according to any one of claims 1-6, characterized in that: The corn cob-derived biomass porous carbon electrode material is a carbon material doped with N, O, F, Cl, P and Zn heteroatoms. It is assembled from nanoparticles and has a rich mesoporous structure.

8. An electrode that uses the corn cob-derived biomass porous carbon electrode material as described in claim 7 as the electrode active material.

9. An aqueous zinc-ion battery, using the electrode as described in claim 8 as the positive electrode.

Citation Information

Patent Citations

  • Nitrogen-doped porous carbon material for lithium ion capacitors, and efficient preparation method thereof through activating biomass waste with low-temperature co-melting solvent

    CN110697708A

  • Preparation method of supercapacitor based on hierarchical pore nitrogen-fluorine doped carbon material working electrode

    CN112687478A

  • Preparation method of nitrogen-doped mesoporous carbon

    CN116654927A