A Ti3C2T X MXene@rGO coaxial fibers, their preparation methods and applications
By preparing Ti₃C₂Tₓ MXene@rGO coaxial fibers, the problems of difficult molding and poor mechanical properties of Ti₃C₂Tₓ MXene fibers have been solved, realizing the high-performance application of flexible conductive fibers, which are suitable for flexible wearable devices.
Patent Information
- Application Number
- CN202410776882.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2024-01-16
- Filing Date
- 2024-06-17
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-06-17
AI Technical Summary
Existing Ti₃C₂Tₓ MXene fibers are difficult to mold, have poor mechanical properties, low energy density, and poor cycle stability, making it difficult to meet the needs of flexible wearable electronic devices.
The coaxial fiber structure of Ti₃C₂Tₓ MXene@rGO is adopted, with the core layer being reduced graphene oxide and the shell layer being Ti₃C₂Tₓ MXene multilayer nanosheets. It is prepared by coaxial wet spinning process and chemical reduction method, and the coagulation bath conditions are optimized to achieve tight bonding and performance improvement of the fibers.
Flexible conductive fibers were fabricated, exhibiting excellent mechanical properties, electrochemical properties, and high energy density, making them suitable for flexible wearable devices and enabling high-performance flexible energy storage applications.
Smart Images

Figure CN118581598B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of flexible energy storage materials, specifically relating to a Ti3C2T X MXene@rGO coaxial fiber anode, its preparation method and application. Background Technology
[0002] With the development of electronic products, especially the emergence of flexible wearable electronic products such as smart glasses, flexible displays, bendable phones, and smart clothing, wearable devices have gained widespread recognition as a focal point of the smart terminal industry. At the same time, these innovative products urgently require high-performance flexible energy storage devices to meet their unique power needs. Flexible solid-state supercapacitors, as a novel type of flexible energy storage device, have attracted much attention due to their outstanding characteristics such as high power, energy density, reliable cycle stability, and safety, making them promising for applications in energy storage systems for flexible electronic products.
[0003] A key factor in the development of flexible solid-state supercapacitors is the performance of their electrode materials. As a cutting-edge representative of flexible energy storage devices, the selection of positive and negative electrode materials is crucial, as they directly affect the capacitor's performance. For advanced two-dimensional transition metal oxide materials such as Ti3C2T... X MXene possesses unique advantages, such as excellent conductivity, high electrochemical performance, and cycle stability, as well as ease of functionalization, making it an outstanding anode material with the potential to match high-performance cathode materials. Therefore, it holds immense promise in the field of flexible energy storage electrodes. However, its problems are also evident: firstly, it is difficult to mold, making it challenging to spin fibers independently; secondly, even if fibers can be spun through controlled processes, the small sheet size and brittle nature of MXene result in extremely poor mechanical properties, failing to meet the demands of practical applications. Therefore, there is a need to develop a flexible conductive fiber to meet the application requirements of wearable electronic devices. Summary of the Invention
[0004] Purpose of the invention: The technical problem to be solved by the present invention is to address the shortcomings of the prior art and provide a Ti3C2T X MXene / rGO coaxial fibers and their preparation methods are proposed to overcome the defects of existing conductive MXene fibers, such as difficult molding, poor mechanical properties, low energy density, and poor cycle stability.
[0005] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0006] A Ti3C2T XMXene@rGO coaxial fiber has a core layer of reduced graphene oxide (rGO) and a shell layer of Ti3C2T. X MXene material, namely titanium carbide (Ti3C2Tx) MXene multilayer nanosheets.
[0007] Specifically, the coaxial fiber has a core diameter of 20–50 μm and a shell diameter of 100–200 μm, with the core and shell tightly connected.
[0008] Furthermore, the present invention also provides the above-mentioned Ti3C2T X The preparation method of MXene@rGO coaxial fibers uses graphene oxide (GO) dispersion as the core spinning solution for the fibers, and Ti3C2T... X MXene dispersion was used as the shell spinning solution for the fiber. Core-shell structures were prepared by coaxial wet spinning of the core and shell spinning solutions, followed by solidification in a coagulation bath to obtain coaxial Ti3C2T. X MXene@GO fibers are then reduced to obtain the final product.
[0009] Furthermore, the aforementioned Ti3C2T X The preparation method of MXene@rGO coaxial fibers specifically includes the following steps:
[0010] (1) Preparation of core layer spinning solution: Graphite oxide is prepared by Hummers method, and then it is separated into layers by mechanical exfoliation and centrifugation to obtain graphene oxide slurry. Finally, it is concentrated to obtain graphene oxide spinning solution.
[0011] (2) Preparation of shell spinning solution: Ti3AlC2MAX was chemically etched to obtain multilayer Ti3C2T X MXene was then subjected to acid washing, water washing, and centrifugation to obtain Ti3C2T. X MXene slurry is then concentrated to obtain shell spinning solution;
[0012] (3) Preparation of coaxial fibers: The core spinning solution and the shell spinning solution were injected into a coagulation bath using a coaxial wet spinning process and solidified to obtain Ti3C2T. X MXene@GO coaxial fiber;
[0013] (4) Chemical reduction: The Ti3C2T obtained in step (3) is chemically reduced. X The MXene@GO coaxial fiber is obtained by chemical reduction.
[0014] Specifically, in step (1), graphene oxide is prepared by flake graphite, and the resulting graphene oxide slurry is concentrated to a concentration of 10 mg / mL to 30 mg / mL, preferably 16 mg / mL.
[0015] Specifically, in step (2), Ti3AlC2MAX is etched with hydrofluoric acid for 24–36 hours, centrifuged at 2000–4000 rpm for 0.5–1 hour to obtain Ti3C2T X The concentration of MXene slurry after concentration is 20 mg / mL to 50 mg / mL, preferably 25 mg / mL.
[0016] Specifically, in step (3), the conditions for the coaxial wet spinning process are as follows: the propulsion speed of the core spinning solution in the coaxial spinning needle is controlled to be 0.2–0.3 mL / min, and the propulsion speed of the shell spinning solution in the coaxial spinning needle is controlled to be 0.5–0.7 mL / min. X The mass ratio of MXene to graphene oxide is 4:1.
[0017] Preferably, the coagulation bath is an aqueous solution of NH4Cl-NH3·H2O with a concentration of 0.5-2 mol / L.
[0018] Take appropriate amounts of the core spinning solution (graphene oxide slurry) and the shell spinning solution (Ti3C2T) using a syringe. X MXene slurry is connected to a coaxial spinning needle (17G+22G, 1.11mm+0.42mm), and then wet spinning is performed by controlling different feed speeds. Finally, the spun fibers are collected and dried.
[0019] Specifically, in step (4), the reducing agent used for chemical reduction is any one of HI, VC or hydrazine hydrate aqueous solution, with a mass concentration of 40-60%, preferably a 55% hydroiodic acid aqueous solution; the constant temperature is 50-80℃, preferably 60℃; and the reduction time is 6-8 hours.
[0020] Furthermore, the present invention also claims protection for the above-mentioned Ti3C2T X Application of MXene@rGO coaxial fibers in the fabrication of asymmetric supercapacitors.
[0021] Specifically, the above-mentioned Ti3C2T X MXene@rGO coaxial fibers were used as the negative electrode of a solid-state supercapacitor, and reduced graphene oxide fibers were used as the positive electrode. The two fibers were parallel to each other, and a 3 mol / L PVA / H2SO4 electrolyte was coated between the two fibers to construct a flexible asymmetric solid-state supercapacitor.
[0022] Beneficial effects:
[0023] (1) This invention improves the existing coaxial fiber system, realizing that when the core material is graphene oxide, the graphene oxide in the core layer can be chemically reduced to impart and improve the overall mechanical and flexible properties of the conductive fiber. The method is simple to operate, the parameters are easy to control, and it can stably and continuously spin out fibers with excellent conductivity and mechanical properties, which has important practical significance.
[0024] (2) This invention uses coaxial spinning to combine the core layer graphene and the shell layer Ti3C2T X The excellent properties of MXene are combined closely. Without affecting the excellent electrochemical performance of the shell, the reduced graphene oxide skeleton of the core layer improves the mechanical properties and flexibility of the coaxial fiber and reduces the stress of the shell layer, thus producing flexible conductive coaxial fibers, which are expected to be used in multifunctional wearable devices, embedded electronic devices and smart fabrics.
[0025] (3) The coagulation bath of this invention also influences the crosslinking and curing of coaxial fibers. The selection and optimization of different coagulation baths determine the structure and properties of coaxial MXene fibers. The core material, shell material, and their interactions directly affect the mechanical properties, electrochemical properties, and stability of the fibers in this process. The NH4Cl-NH3·H2O coagulation bath performs excellently in the construction and properties of coaxial fibers. It not only helps to quickly construct coaxial structures but also achieves optimal mechanical and electrochemical properties.
[0026] (4) The core layer of this invention uses Ti3C2T X MXene provides ultra-high electrochemical performance and abundant ion-accessible sites on its surface, thus enabling the prepared conductive coaxial fibers to possess both excellent electrochemical and mechanical properties.
[0027] (5) This invention relates to Ti3C2T X The preparation method of MXene-coated reduced graphene oxide coaxial fiber anode and supercapacitor can achieve the control of the mechanical and electrical properties of coaxial fibers by adjusting the concentration of the core-shell spinning solution, the parameters of the coaxial spinning needle, the spinning rate ratio, and the type of coagulation bath.
[0028] (6) The coaxial Ti3C2Tx@rGO fiber of this invention has an electrical conductivity of 15645.1 S / m. Under the conditions of liquid three electrodes and 3M H2SO4, the optimal voltage window of this flexible fiber is -0.9 to -0.1 V. At a current density of 1 A / g, the specific capacitance of this electrode is as high as 452 F / g. In the mechanical test of the fiber, the tensile strength of the fiber reaches 95 MPa, proving that this fiber is a negative electrode material with both performance and strength, and has excellent application potential as a flexible negative electrode in the field of smart wearable devices. Attached Figure Description
[0029] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments, and the advantages of the present invention in the above and / or other aspects will become clearer.
[0030] Figure 1 This is a schematic diagram of the coaxial wet spinning process of the present invention.
[0031] Figure 2 This is a photograph of the coaxial wet spinning needle of the present invention.
[0032] Figure 3 This is a schematic diagram of the coaxial fiber structure of the present invention.
[0033] Figure 4 The coaxial Ti3C2T of this invention X Image of MXene@reduced graphene oxide fiber.
[0034] Figure 5 Coaxial Ti3C2T X Cross-sectional scanning electron microscope image of MXene@reduced graphene oxide fibers.
[0035] Figure 6 Coaxial Ti3C2T X XRD comparison of MXene@reduced graphene oxide fibers.
[0036] Figure 7 Coaxial Ti3C2T X Raman comparison of MXene@reduced graphene oxide fibers.
[0037] Figure 8 Coaxial Ti3C2T X Cyclic voltammetric properties of MXene@reduced graphene oxide fibers at different scan rates.
[0038] Figure 9 Coaxial Ti3C2T X Constant current charge-discharge performance of MXene@reduced graphene oxide fibers at different current densities.
[0039] Figure 10 Coaxial Ti3C2T X EIS impedance diagram of MXene@reduced graphene oxide fibers.
[0040] Figure 11 Coaxial Ti3C2T X Comparison of specific capacitance of MXene@reduced graphene oxide fibers at different current densities.
[0041] Figure 12 Coaxial Ti3C2T X The capacitance retention rate of MXene@reduced graphene oxide fiber after 10,000 charge-discharge cycles.
[0042] Figure 13 Coaxial Ti3C2T X Comparison of mechanical properties of MXene@reduced graphene oxide fibers.
[0043] Figure 14 Coaxial Ti3C2T X Stress simulation diagram of MXene@reduced graphene oxide fiber under stress in the middle and at both ends.
[0044] Figure 15 This is a comparison of capacitance retention rates of coaxial fiber-based supercapacitors after 2000 bending cycles.
[0045] Figure 16 This is a diagram showing the structure and application of a coaxial fiber-based supercapacitor.
[0046] Figure 17 The effect of different coagulation baths on fiber forming effect: (a) anhydrous ethanol, (b) 0.5M CTAB solution, (c) 0.5M CaCl2 solution, (d) 0.5M NH4Cl-NH3·H2O solution. Detailed Implementation
[0047] The present invention can be better understood from the following embodiments.
[0048] This invention prepares flexible coaxial structure fibers through coaxial spinning. Compared with the layer-by-layer assembly of hybrid fibers, the coaxial structure can improve mechanical properties without destroying the conductive network structure of MXene material, thus maintaining the high conductivity of the fiber.
[0049] Figure 1 This is a schematic diagram of the coaxial wet spinning process of the present invention, using graphene oxide dispersion as the core spinning solution for the fiber, and Ti3C2T... X MXene dispersion was used as the shell spinning solution for fibers. Appropriate amounts of the core spinning solution (graphene oxide slurry) and the shell spinning solution (Ti3C2T) were taken separately using a syringe.X MXene slurry was connected to a coaxial spinning needle (17G+22G, 1.11mm+0.42mm), and then wet spinning was performed by controlling different feed speeds. The slurry was then cured in a coagulation bath to obtain coaxial Ti3C2T. X MXene@GO fiber is then collected and dried.
[0050] The coaxial spinning needle used in this invention is as follows: Figure 2 As shown, the shell and core needle form a coaxial structure. The shell diameter is 1.04mm and the core diameter is 0.41mm. The needle was purchased from Xindong dispensing equipment, model number 17G+22G.
[0051] Figure 3 The present invention is Ti3C2T X A schematic diagram of MXene@rGO coaxial fiber, with a core layer of reduced graphene oxide and a shell layer of titanium carbide (Ti3C2Tx)MXene multilayer nanosheets. The core layer diameter of the coaxial fiber is 20–50 μm, and the shell layer diameter is 100–200 μm, with the core and shell layers tightly connected.
[0052] The core layer is made of carbon material with excellent mechanical properties and high spinnability to provide skeletal support, while the shell layer is made of MXene material with strong electrochemical properties and abundant surface ion sites, thus endowing the coaxial fiber with excellent properties such as flexibility, mechanical and electrochemical properties, and easy forming and processing.
[0053] Example 1
[0054] The fiber is a shell-type Ti3C2T. X A coaxial structure of MXene-encapsulated core layer of reduced graphene oxide is constructed. This coaxial fiber is then assembled with reduced graphene oxide fibers to form a solid-state asymmetric supercapacitor. The specific preparation method includes the following steps:
[0055] (1) 3g of graphite powder was used to prepare graphene oxide by the Hummers method, and then graphene oxide slurry with a concentration of 16mg / mL was obtained by mechanical exfoliation and centrifugation.
[0056] (2) Take 2g of lithium fluoride and 40ml of hydrochloric acid, react at 35℃ for half an hour, then add 2g of Ti3AlC2 MAX phase and etch for 36 hours. Finally, take it out, and after acid washing and water washing, obtain a monolayer or few-layer Ti3C2T with a pH greater than 5. X MXene. MXene was concentrated to 25 mg / mL by centrifugation;
[0057] (3) Take 5 mL of graphene oxide slurry and Ti3C2T X10 mL of MXene slurry was added to the syringe, and the spinning solution was passed through a coaxial spinning needle (17G+22G) with an outer inner diameter of 1.04 mm and an inner inner diameter of 0.41 mm. Figure 2 As shown. Graphene oxide slurry was injected into the core layer at an injection rate of 0.2 mL / min, Ti3C2T X MXene slurry was introduced into the shell layer at an injection rate of 0.5 mL / min and injected into the coagulation bath, which was a 0.5 M NH4Cl-NH3·H2O aqueous solution. The fibers formed well in the NH4Cl-NH3·H2O aqueous solution and were relatively easy to remove from the coagulation bath.
[0058] (4) After half an hour, once the coaxial fiber has solidified, it is placed in a hydroiodic acid solution with a mass fraction of approximately 55% for reduction. The hydroiodic acid must completely cover the fiber. After reduction at 60°C for 8 hours, the fiber is washed and dried to obtain coaxial Ti3C2T. X MXene@reduced graphene oxide fibers, such as Figure 4 As shown.
[0059] (5) Take the coaxial Ti3C2T obtained in step (4) X @rGO fiber and a reduced graphene oxide fiber are placed parallel to each other on a PET film. The two fibers are coated with an electrolyte and then fixed at both ends with conductive silver paste. After natural drying, a fiber-based asymmetric supercapacitor is obtained. This yields an asymmetric coaxial fiber supercapacitor.
[0060] Figure 4 This embodiment uses Ti3C2T. X Actual photos of MXene@rGO coaxial fibers. Figure 5 This embodiment uses Ti3C2T. X Cross-sectional scanning electron microscope image of MXene@rGO coaxial fiber. Combined with... Figure 4 and Figure 5 It can be seen that the prepared Ti3C2T X MXene@rGO fibers have a coaxial structure, with the outermost layer being Ti3C2T. X MXene has an rGO core layer, and the two are tightly connected.
[0061] Figure 6 This embodiment uses Ti3C2T. X XRD patterns of MXene@rGO coaxial fibers show that Ti3C2T was successfully prepared from the Ti3AlC2MAX phase. XIn MXene fibers, the characteristic peak of the MAX phase at 39° disappears, while MXene shows a (002) peak at 7°. After coaxial composite with graphene oxide (GO), the XRD pattern of MXene@GO fibers shows a (002) peak of graphene oxide, indicating successful composite of GO and MXene. Following chemical reduction, in MXene@rGO fibers, the (002) peak of GO disappears with reduction, and the graphite peak becomes more prominent. Simultaneously, when combined with graphene oxide, the (002) peak of MXene shifts to a smaller angle, indicating an intercalation effect between MXene and graphene oxide.
[0062] Figure 7 This embodiment uses Ti3C2T. X Raman comparison of MXene@rGO coaxial fibers. The peak at 194 cm⁻¹ corresponds to the A1g vibration of Ti, while the peaks at 274, 367, and 624 cm⁻¹ correspond to the vibrations of Ti. -1 The peak value at this point corresponds to the Eg-based vibration, indicating that MXene nanosheets are embedded in rGO. Furthermore, Ti3C2T X MXene@GO fiber I D / I G The ratio is 0.87, while after chemical reduction with HI acid, Ti3C2T X MXene@rGO fiber I D / I G The ratio increased to 0.96. D / I G The increase in the degree of defects indicates an increase in the amount of active sites provided for the electrolyte, thereby improving the electrochemical performance of the material.
[0063] Figure 8 This embodiment uses Ti3C2T. X Electrochemical testing was performed on the MXene@rGO coaxial fiber three-electrode system, with cyclic voltammetry curves at scan rates ranging from 2 to 50 mV / s. At different scan rates, the CV curves exhibited an approximately rectangular shape, indicating that the material possesses excellent stability and rate performance. Figure 9 This embodiment of Ti3C2T is shown. X The constant current charge-discharge curves of MXene@rGO coaxial fibers at current densities ranging from 1 to 10 A / g are shown. The charge-discharge curves exhibit an approximately isosceles triangular shape, indicating excellent electrochemical reversibility even at high current densities. Figure 10 This embodiment uses Ti3C2T. X MXene@rGO coaxial fibers at 0.01Hz to 10 5Electrochemical impedance spectroscopy (EIS) within the Hz frequency range reveals a low internal resistance of 5 Ω in the high-frequency region, indicating good electrical conductivity. The low-frequency region also shows a steeper slope in the fiber curve, suggesting a faster charge diffusion rate, contributing to the excellent electrochemical performance of the coaxial fibers. Figure 11 This embodiment uses Ti3C2T. X The specific capacitance of MXene@rGO coaxial fiber at current densities ranging from 1 to 20 A / g, with a maximum specific capacitance of 452 F / g at a current density of 1 A / g. Figure 12 This embodiment uses Ti3C2T. X After 10,000 charge-discharge cycles, the MXene@rGO coaxial fiber electrode retained 94% of its capacity, indicating excellent cycle stability. At a current density of 0.1 A / g, the assembled solid-state supercapacitor exhibited a specific capacitance of 243 F / g. Furthermore, according to E = 1 / 2CV... 2 Its energy density can be as high as 68Wh / Kg.
[0064] Figure 13 This embodiment uses Ti3C2T. X MXene@rGO coaxial fiber and Ti3C2T X Comparison of mechanical properties of MXene / rGO blended fibers and MXene fibers, coaxial Ti3C2T X The mechanical properties of MXene@rGO fiber are 95 MPa, which is 167% of that of MXene / rGO fiber and 413% of that of pure MXene fiber, demonstrating the advantages of coaxial fiber.
[0065] Figure 14 This demonstrates the use of COMSOL software to integrate a coaxial Ti3C2T X Stress simulations of MXene / reduced graphene oxide fibers and rGO fibers under stress at the middle and both ends show that stress in the coaxial fibers is concentrated in the mechanically strong rGO core layer, thereby reducing the stress on Ti3C2T. X The stress on the MXene surface effectively protects the fragile MXene, achieving a coordinated development of electrical and mechanical properties.
[0066] Figure 15 The capacitance retention rate of the coaxial fiber-based solid-state supercapacitor and the MXene fiber-based supercapacitor after 2000 bending cycles is as high as 93.67%, compared to 45.10% for the MXene fiber-based supercapacitor after 2000 bending cycles. This indicates that the coaxial fiber electrode has excellent flexibility in terms of bending resistance.
[0067] Coaxial fiber-based solid-state supercapacitors can provide energy densities of 30.1 to 68.1 Wh / kg at power densities of 1.2 to 12 kW / kg, while also exhibiting a tensile strength of 95 MPa, achieving synergistic development of mechanical and electrochemical properties. To evaluate the feasibility of coaxial fiber flexible supercapacitors in practical applications, this invention utilizes these fiber electrodes to fabricate a chip-structured supercapacitor. For example... Figure 16 As shown, the system successfully powered LED lights, a small fan, a flexible LED screen, and a heart rate and blood pressure sensor. This demonstrates that the coaxial fiber-based flexible supercapacitor possesses excellent energy storage performance, significant mechanical flexibility, and series-parallel output characteristics, making it valuable for applications in the field of new energy storage.
[0068] Example 2
[0069] The fiber is a shell-type Ti3C2T. X A coaxial structure of MXene-encapsulated core layer of reduced graphene oxide is formed. This coaxial fiber is then assembled with reduced graphene oxide fibers to create a solid-state asymmetric supercapacitor. The specific preparation method includes the following steps:
[0070] (1) 3g of graphite powder was used to prepare graphene oxide by the Hummers method, and then graphene oxide slurry with a concentration of 18mg / mL was obtained by mechanical exfoliation and centrifugation.
[0071] (2) Take 2g of lithium fluoride and 40ml of hydrochloric acid, react at 35℃ for half an hour, then add 2g of Ti3AlC2 MAX phase and etch for 36 hours. Finally, take it out, and after acid washing and water washing, obtain a monolayer or few-layer Ti3C2T with a pH greater than 5. X MXene. MXene was concentrated to 25 mg / mL by centrifugation;
[0072] (3) Take 5 mL of graphene oxide slurry and Ti3C2T X 10 mL of MXene slurry was added to the syringe, and the spinning solution was passed through a coaxial spinning needle (17G+22G) with an outer inner diameter of 1.04 mm and an inner inner diameter of 0.41 mm. Figure 3 As shown. Graphene oxide slurry was injected into the core layer at an injection rate of 0.2 mL / min, Ti3C2T X MXene slurry was introduced into the shell layer at an injection rate of 0.5 mL / min and injected into the coagulation bath, which was a 0.5 mol / L NH4Cl-NH3·H2O aqueous solution.
[0073] (4) After half an hour, once the coaxial fiber has solidified, it is placed in a hydroiodic acid solution with a mass fraction of approximately 55% for reduction. The hydroiodic acid must completely cover the fiber. After reduction at 60°C for 8 hours, coaxial Ti3C2T is obtained. X MXene@reduced graphene oxide fiber;
[0074] (5) Take the coaxial Ti3C2T obtained in step (4) X @rGO fiber and a reduced graphene oxide fiber are placed parallel to each other on a PET film. The two fibers are coated with an electrolyte and then fixed at both ends with conductive silver paste. After natural drying, a fiber-based asymmetric supercapacitor is obtained. This yields an asymmetric coaxial fiber supercapacitor.
[0075] Example 3
[0076] The fiber is a shell-type Ti3C2T. X A coaxial structure of MXene-encapsulated core layer of reduced graphene oxide is formed. This coaxial fiber is then assembled with reduced graphene oxide fibers to create a solid-state asymmetric supercapacitor. The specific preparation method includes the following steps:
[0077] (1) 3g of graphite powder was used to prepare graphene oxide by the Hummers method, and then graphene oxide slurry with a concentration of 12mg / mL was obtained by mechanical exfoliation and centrifugation.
[0078] (2) Take 2g of lithium fluoride and 40ml of hydrochloric acid, react at 35℃ for half an hour, then add 2g of Ti3AlC2 MAX phase and etch for 36 hours. Finally, take it out, and after acid washing and water washing, obtain a monolayer or few-layer Ti3C2T with a pH greater than 5. X MXene. MXene was concentrated to 25 mg / mL by centrifugation;
[0079] (3) Take 5 mL of graphene oxide slurry and Ti3C2T X 10 mL of MXene slurry was added to the syringe, and the spinning solution was passed through a coaxial spinning needle (17G+22G) with an outer inner diameter of 1.04 mm and an inner inner diameter of 0.41 mm. Figure 3 As shown. Graphene oxide slurry was injected into the core layer at an injection rate of 0.2 mL / min, Ti3C2T X MXene slurry was introduced into the shell layer at an injection rate of 0.5 mL / min and injected into the coagulation bath, which was a 0.5 mol / L NH4Cl-NH3·H2O aqueous solution.
[0080] (4) After half an hour, the coaxial fiber solidifies and is then placed in a hydroiodic acid solution with a mass fraction of about 55% for reduction. The hydroiodic acid needs to cover the fiber. After reduction at 60°C for 8 hours, coaxial Ti3C2Tx MXene@reduced graphene oxide fiber is obtained.
[0081] (5) Take the coaxial Ti3C2T obtained in step (4) X @rGO fiber and a reduced graphene oxide fiber are placed parallel to each other on a PET film. The two fibers are coated with an electrolyte and then fixed at both ends with conductive silver paste. After natural drying, a fiber-based asymmetric supercapacitor is obtained. This yields an asymmetric coaxial fiber supercapacitor.
[0082] Comparative Example 1
[0083] (1) 3g of graphite powder was used to prepare graphene oxide by the Hummers method, and then graphene oxide slurry with a concentration of 16mg / mL was obtained by mechanical exfoliation and centrifugation.
[0084] (2) Take 2g of lithium fluoride and 40ml of hydrochloric acid, react at 35℃ for half an hour, then add 2g of Ti3AlC2 MAX phase and etch for 36 hours. Finally, take it out, and after acid washing and water washing, obtain monolayer or few-layer Ti3C2Tx MXene with pH greater than 5. Concentrate MXene to 25mg / mL by centrifugation;
[0085] (3) Take 5 mL of graphene oxide slurry and 10 mL of Ti3C2Tx MXene slurry, add the above spinning solutions into syringes respectively, and pass them through coaxial spinning needles (17G+22G) with an outer inner diameter of 1.04 mm and an inner inner diameter of 0.41 mm. Figure 3 As shown. Graphene oxide slurry was injected into the core layer at an injection rate of 0.2 mL / min, Ti3C2T X MXene slurry was introduced into the shell layer at an injection rate of 0.5 mL / min and injected into the coagulation bath.
[0086] The coagulation baths used were anhydrous ethanol, 0.5M CTAB, 0.5M CaCl2 solution, and 0.5M NH4Cl-NH3·H2O. The effects of using different coagulation bath methods are as follows: Figure 17 As shown.
[0087] When anhydrous ethanol is used as the coagulation bath, most of the fibers dissolve in the ethanol coagulation bath, see [reference needed]. Figure 17 a indicates that the ethanol coagulation bath is not suitable for this system, and another type of coagulation bath should be used instead. When the coagulation bath is 0.5M CTAB, unlike in the ethanol coagulation bath, the fibers do not dissolve, but instead appear as bead-like structures and cannot form fibers. See [link to relevant documentation]. Figure 17b indicates that CTAB is also unsuitable for this system; other coagulation baths should be used instead. When the coagulation bath is a 0.5M CaCl2 solution, the fibers can be formed in the CaCl2 coagulation bath, but the continuity is poor, the flexibility is poor, the surface is rough, and it is difficult to pick them out of the coagulation bath. See [link to relevant documentation]. Figure 17 c. When the coagulation bath is a 0.5M NH4Cl-NH3·H2O aqueous solution, the fibers form well in the NH4Cl-NH3·H2O aqueous solution and are relatively easy to remove from the coagulation bath. See Figure 17 d indicates that the NH4Cl-NH3·H2O coagulation bath is a suitable coagulation bath.
[0088] Comparative Example 2
[0089] (1) Take 2g of lithium fluoride and 40ml of hydrochloric acid, react at 35℃ for half an hour, then add 2g of Ti3AlC2 MAX phase and etch for 36 hours. Finally, take it out, and after acid washing and water washing, obtain a monolayer or few-layer Ti3C2T with pH greater than 5. X MXene. MXene was concentrated to 25 mg / mL by centrifugation;
[0090] (2) Take 10 mL of the above spinning solution and add it into a syringe. Then, inject it into the coagulation bath through a 17G spinning needle at a speed of 0.5 mL / min. The coagulation bath is a 0.5 mol / L NH4Cl-NH3·H2O aqueous solution.
[0091] (3) After half an hour, once the coaxial fiber has solidified, it is placed in a hydroiodic acid solution with a mass fraction of approximately 55% for reduction. The hydroiodic acid must completely cover the fiber. After reduction at 60°C for 8 hours, pure Ti3C2T is obtained. X MXene fibers;
[0092] Ti3C2T X MXene fiber achieves a specific capacitance of 480 F / g at a current density of 1 A / g, but its mechanical properties are only 23 MPa, which affects its practical applications.
[0093] Comparative Example 3
[0094] (1) 3g of graphite powder was used to prepare graphene oxide by the Hummers method, and then graphene oxide slurry with a concentration of 16mg / mL was obtained by mechanical exfoliation and centrifugation.
[0095] (2) Take 2g of lithium fluoride and 40ml of hydrochloric acid, react at 35℃ for half an hour, then add 2g of Ti3AlC2 MAX phase and etch for 36 hours. Finally, take it out, and after acid washing and water washing, obtain monolayer or few-layer Ti3C2Tx MXene with pH greater than 5. Concentrate MXene to 25mg / mL by centrifugation;
[0096] (3) Take 5 mL of graphene oxide slurry and 10 mL of Ti3C2Tx MXene slurry, mix them thoroughly, add them to a syringe, and inject them into a coagulation bath through a 17G spinning needle at an injection speed of 0.5 mL / min. The coagulation bath is a 0.5 mol / L NH4Cl-NH3·H2O aqueous solution.
[0097] Ti3C2T X MXene and reduced graphene oxide blended fibers exhibit a specific capacitance of only 386 F / g and a mechanical strength of 56 MPa at a current density of 1 A / g, both lower than those of coaxial Ti3C2T. X MXene@rGO fiber.
[0098] This invention provides a Ti3C2T X The present invention relates to MXene@rGO coaxial fibers, their preparation methods, and applications. Many methods and approaches exist for implementing this technical solution. The above description is merely a preferred embodiment of the invention. It should be noted that those skilled in the art can make various improvements and modifications without departing from the principles of the invention, and these improvements and modifications should also be considered within the scope of protection of the invention. All components not explicitly described in this embodiment can be implemented using existing technologies.
Claims
1. A Ti3C2T X MXene@rGO coaxial fiber, characterized in that, Its core layer is made of reduced graphene oxide, and its shell layer is made of Ti3C2T. X MXene material.
2. The Ti3C2T according to claim 1 X MXene@rGO coaxial fiber, characterized in that, The coaxial fiber has a core diameter of 20-50 µm and a shell diameter of 100-200 µm, with the core and shell tightly connected.
3. The Ti3C2T as described in claim 1 X The method for preparing MXene@rGO coaxial fibers is characterized by, Using graphene oxide dispersion as the core spinning solution for fibers, and Ti3C2T X MXene dispersion was used as the shell spinning solution for the fiber. Core-shell structures were prepared by coaxial wet spinning of the core and shell spinning solutions, followed by solidification in a coagulation bath to obtain coaxial Ti3C2T. X MXene@GO fiber is obtained by reduction; the coagulation bath is an aqueous solution of NH4Cl-NH3·H2O with a concentration of 0.5-2 mol / L.
4. The Ti3C2T according to claim 3 X The method for preparing MXene@rGO coaxial fibers is characterized by, Specifically, the steps include the following: (1) Preparation of core layer spinning solution: Graphite oxide is prepared by Hummers method, and then it is separated into layers by mechanical exfoliation and centrifugation to obtain graphene oxide slurry. Finally, it is concentrated to obtain graphene oxide spinning solution. (2) Preparation of shell spinning solution: Ti3AlC2MAX was chemically etched to obtain multilayer Ti3C2T X MXene was then subjected to acid washing, water washing, and centrifugation to obtain Ti3C2T. X MXene slurry is then concentrated to obtain shell spinning solution; (3) Preparation of coaxial fibers: The core spinning solution and the shell spinning solution are injected into the coagulation bath through a coaxial wet spinning process using a coaxial spinning needle, and then solidified to obtain Ti3C2T X MXene@GO coaxial fiber; (4) Chemical reduction: The Ti3C2T obtained in step (3) is chemically reduced. X The MXene@GO coaxial fiber is obtained by chemical reduction.
5. The Ti3C2T according to claim 4 X The method for preparing MXene@rGO coaxial fibers is characterized by, In step (1), graphene oxide is prepared by flake graphite, and the resulting graphene oxide slurry is concentrated to a concentration of 10 mg / mL to 30 mg / mL.
6. The Ti3C2T according to claim 4 X The method for preparing MXene@rGO coaxial fibers is characterized by, In step (2), Ti3AlC2MAX is etched with lithium fluoride and hydrochloric acid for 24–36 hours, centrifuged at 2000–4000 rpm for 0.5–1 hour to obtain Ti3C2T. X The concentration of MXene slurry after concentration is 20 mg / mL to 50 mg / mL.
7. The Ti3C2T according to claim 4 X The method for preparing MXene@rGO coaxial fibers is characterized by, In step (3), the conditions for the coaxial wet spinning process are as follows: the propulsion speed of the core spinning solution in the coaxial spinning needle is controlled to be 0.2~0.3 mL / min, and the propulsion speed of the shell spinning solution in the coaxial spinning needle is controlled to be 0.5~0.7 mL / min.
8. The Ti3C2T according to claim 4 X The method for preparing MXene@rGO coaxial fibers is characterized by, In step (4), the reducing agent used for chemical reduction is an aqueous solution of HI with a mass concentration of 40~60wt%; the constant temperature is 50~80℃ and the reduction time is 6~8 hours.
9. The Ti3C2T according to claim 1 X Application of MXene@rGO coaxial fibers in the fabrication of asymmetric supercapacitors.
Citation Information
Patent Citations
MXene / rGO (at) SA coaxial composite fiber based on core-shell structure as well as preparation method and application of MXene / rGO (at) SA coaxial composite fiber
CN120925114A
Core-shell structure optical phase filler, radiation refrigeration coating as well as preparation method and application of core-shell structure optical phase filler and radiation refrigeration coating
CN122772417A