A catalytic structure for reducing the amount of ozone in a plasma generating device, a low-ozone plasma generating device and applications thereof

By using honeycomb ceramics loaded with CuMnCeOx catalyst in a plasma generator, combined with a dielectric barrier discharge structure, ozone can be directly decomposed and converted, solving the problems of complex structure and high cost of plasma generators, and achieving low ozone concentration and efficient sterilization.

CN118594559BActive Publication Date: 2026-11-20GREE ELECTRIC APPLIANCE INC OF ZHUHAI
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410638910.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-22
Publication Date
2026-11-20
Estimated Expiration
2044-05-22

AI Technical Summary

Technical Problem

Existing plasma generators are complex in structure, expensive, and have difficulty controlling ozone concentration, resulting in poor sterilization effect or exceeding the standard.

Method used

Using honeycomb ceramics loaded with CuMnCeOx catalyst, combined with a needle-plate electrode structure for dielectric barrier discharge, ozone is directly decomposed in the plasma generation region and converted into highly oxidizing superoxide radicals.

Benefits of technology

It achieves stable reduction of ozone concentration to a safe range with low cost and simple structure, while improving sterilization efficiency and ensuring highly effective microbial disinfection.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118594559B_ABST
    Figure CN118594559B_ABST
Patent Text Reader

Abstract

The application discloses a catalytic structure for reducing the amount of ozone of a sub-plasma generating device, a low-ozone plasma generating device and application thereof, and relates to a low-ozone plasma generating device, which comprises a plasma generating device for generating ozone; and a honeycomb ceramic loaded with a CuMnCeOx catalyst, which is arranged in a plasma generating area of the plasma generating device. The application can synchronously and stably decompose ozone in real time, reduce the content of ozone to a safe concentration range, and decompose the ozone into active substances such as hydroxyl radicals and superoxide free radicals, so that the ozone release is reduced, and the multiple effects of the active substances and the plasma electric field force are utilized to ensure high-efficiency microbial disinfection and sterilization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of plasma sterilization, specifically to a catalytic structure for reducing ozone levels in plasma generators, a low-ozone plasma generator, and its applications. Background Technology

[0002] Plasma, as the fourth state of matter, contains various high-energy particles that can be used for sterilization, with ozone playing a primary role. Insufficient ozone concentration results in poor sterilization. To achieve ideal sterilization, a higher input voltage is often required, typically achieved through high-voltage discharge to generate plasma. However, high-voltage ionization of air produces a large amount of ozone. This method is energy-intensive, and the resulting ozone concentration far exceeds safe levels, severely limiting its further applications.

[0003] To address the problem of excessive ozone concentrations, discharge voltage is typically controlled to reduce ozone production. However, controlling the ozone level is difficult, and it often falls below the sterilization concentration, resulting in a significant reduction in sterilization performance. Therefore, the conventional approach is to add an ozone reduction grid after the plasma generator to decompose ozone concentrations exceeding the safety limit, thus meeting safety requirements while maintaining sterilization effectiveness. However, this method increases costs.

[0004] Currently, existing technology CN 112294991A discloses a method that utilizes the reaction between mist generated by an atomizing module and plasma to produce highly oxidizing active particles, thereby reducing ozone concentration and improving sterilization rate. This existing technology addresses ozone concentration by reacting the ozone after mixing in the external sterilization space. However, the ozone concentration in the external space is unstable, requiring real-time monitoring of ozone and mist levels within the sterilization space to ensure stability. For example, Chinese patent document CN 117357673 A discloses that activating the heating module and / or fan and / or steam module can effectively accelerate the decomposition of ozone in the sterilization chamber, reducing the ozone concentration to a acceptable level at the end of sterilization, thus avoiding harm to the human body. The methods disclosed in these documents require additional equipment such as ozone concentration monitoring and controllers for adjusting the parameters of the heating module and / or fan and / or steam module, resulting in complex structures and increased production costs. Summary of the Invention

[0005] Therefore, the technical problem to be solved by the present invention is that the plasma generating devices in the prior art have defects such as complex structure and high cost, thereby providing a catalytic structure for reducing the ozone content of plasma generating devices, a low-ozone plasma generating device and its application.

[0006] A catalytic structure for reducing ozone levels in an ion generator is a honeycomb ceramic supported on a CuMnCeOx catalyst.

[0007] The molar ratio of Mn, Ce, and Cu in the CuMnCeOx catalyst is 5:2:1.

[0008] The loading of CuMnCeOx catalyst in the honeycomb ceramic is 10-20 wt.%.

[0009] The loading of CuMnCeOx catalyst in the honeycomb ceramic is 15 wt.%.

[0010] The porosity of the honeycomb ceramic is 40-60%, and / or the pore size of the honeycomb ceramic is 10-20 μm.

[0011] The preparation method of the above-mentioned catalytic structure for reducing ozone content in an ion generator includes:

[0012] Precursor salts of Mn, Ce, and Cu were obtained and dissolved in deionized water to obtain a precursor mixture.

[0013] The precursor mixture was subjected to a hydrothermal reaction.

[0014] After the hydrothermal reaction is complete, wash, filter, and perform the first drying.

[0015] The CuMnCeOx catalyst was obtained by calcination after the first drying.

[0016] The CuMnCeOx catalyst was ground to below 200 mesh and added to the binder solution to form a slurry;

[0017] The honeycomb ceramic is mixed with a slurry to allow the slurry to adhere to the honeycomb ceramic. After a second drying, a honeycomb ceramic loaded with a CuMnCeOx catalyst is obtained.

[0018] The mass ratio of CuMnCeOx catalyst to binder in the binder solution is (2.5-3.5):1.

[0019] The precursor salt of Mn is at least one of potassium permanganate, manganese nitrate, and manganese acetate;

[0020] The precursor salt of Ce is at least one of cerium nitrate and cerium oxide;

[0021] The precursor salt of Cu is at least one of copper nitrate and copper sulfate.

[0022] The hydrothermal reaction is carried out at a temperature of 100–150°C for 10–15 hours.

[0023] And / or, the first drying method is: overnight drying at 80℃~120℃;

[0024] And / or, the calcination temperature is 400℃~600℃, the calcination time is 2~4h, and the heating rate is 2~5℃ / min;

[0025] And / or, the honeycomb ceramic is impregnated in a slurry to allow the slurry to adhere;

[0026] And / or, the temperature for the second drying is 100–150°C.

[0027] The soaking time is 5 minutes or more.

[0028] A low-ozone plasma generator, comprising:

[0029] A plasma generator used to produce ozone;

[0030] The aforementioned honeycomb ceramic loaded with CuMnCeOx catalyst is placed in the plasma generation region of the plasma generator.

[0031] The plasma generator is a needle-plate electrode structure with dielectric barrier discharge.

[0032] Application of the aforementioned low-ozone plasma generator in converting ozone into highly oxidizing superoxide radicals.

[0033] The technical solution of this invention has the following advantages:

[0034] 1. This invention provides a catalytic structure for reducing ozone levels in a plasma generator. The structure is a honeycomb ceramic supported on a CuMnCeOx catalyst. When applied to the plasma generation region of the plasma generator, it not only generates ozone, but also, due to the large surface defects of the CuMnCeOx catalyst and the excellent high-temperature stability of the honeycomb ceramic supported on the CuMnCeOx catalyst, it can simultaneously and stably decompose ozone in real time, reducing the ozone content to a safe concentration range and decomposing ozone into reactive substances such as hydroxyl groups and superoxide radicals, for example, highly oxidizing O2. - / O2 2- O2 - / O2 2- While reducing ozone release, it utilizes the combined effects of active substances and plasma electric field force to ensure highly efficient microbial disinfection.

[0035] 2. The low-ozone plasma generator provided by this invention adopts a combination of honeycomb catalysis technology and plasma technology. That is, the plasma generator is used in conjunction with honeycomb ceramic loaded with CuMnCeOx catalyst. The honeycomb ceramic loaded with CuMnCeOx catalyst is placed in the plasma generation area of ​​the plasma generator. No additional devices or equipment are required. With a simpler structure and lower cost, it can achieve a stable and continuous reduction in ozone release from the plasma while achieving a highly efficient microbial killing effect.

[0036] 3. This invention provides a low-ozone plasma generator, wherein the plasma generator is preferably a needle-plate electrode structure of dielectric barrier discharge (DBD). Dielectric barrier discharge is commonly used to generate plasma due to its simple structure and relatively low energy consumption, and is one of the most commonly used discharge methods. Needle-plate DBD discharge is very common, with a simple structure and rapid heat dissipation. When the voltage between the two electrodes is high enough, the discharge gap will break down, forming a gas discharge, which can be used for disinfection and sterilization. However, its disadvantage is a high ozone concentration. This invention utilizes a needle-plate electrode structure of dielectric barrier discharge combined with honeycomb ceramic loaded with a CuMnCeOx catalyst. This allows for the simultaneous decomposition of ozone at the ozone generation location, reducing the ozone concentration. No additional equipment is required to stably ensure that the ozone concentration is reduced to a safe range. Furthermore, placing the honeycomb ceramic in the plasma drift region of the needle-plate discharge structure allows for real-time conversion of the generated ozone into O2. - / O2 2- O2 - / O2 2- It has strong oxidizing properties, which can reduce ozone release and make up for the lack of disinfection performance, thus achieving a better microbial disinfection effect. Attached Figure Description

[0037] To more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the drawings used in the description of the specific embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For those skilled in the art, other drawings can be obtained from these drawings without creative effort.

[0038] Figure 1 This is a schematic diagram of the low-ozone plasma generator in this invention;

[0039] Figure label:

[0040] 1-Plasma generator; 2-Honeycomb ceramic supported on CuMnCeOx catalyst. Detailed Implementation

[0041] The following embodiments are provided to better understand the present invention and are not limited to the preferred embodiments described. They do not constitute a limitation on the content and scope of protection of the present invention. Any product that is the same as or similar to the present invention, derived by any person under the guidance of the present invention or by combining the features of the present invention with other prior art, falls within the protection scope of the present invention.

[0042] For experiments not specifically described in the examples, the procedures or conditions should be followed according to the conventional experimental procedures described in the literature in this field. Reagents or instruments whose manufacturers are not specified are all commercially available conventional reagent products.

[0043] Example 1

[0044] A low-ozone plasma generator, such as Figure 1 As shown, the device includes a plasma generator 1 and a honeycomb ceramic 2 loaded with a CuMnCeOx catalyst. The plasma generator 1 is a needle-plate electrode structure with dielectric barrier discharge. The honeycomb ceramic 2 loaded with the CuMnCeOx catalyst is placed within the plasma region of the plasma generator 1. Figure 1 Within the drift area marked by the dashed line, applying high pressure can achieve low ozone release and good sterilization effect. This device is simple and efficient to use.

[0045] The preparation method of honeycomb ceramics supported on CuMnCeOx catalyst is as follows:

[0046] ① Weigh out the Mn precursor, Ce precursor, and Cu precursor in a molar ratio of 5:2:1 and dissolve them in deionized water; wherein the Mn precursor is potassium permanganate, the Ce precursor is cerium nitrate, and the Cu precursor is copper nitrate.

[0047] ② Transfer the mixture to a hydrothermal reactor and react at 130°C for 12 hours;

[0048] ③ Wash and filter, then dry overnight at 100℃;

[0049] ④ The catalyst sample was obtained by calcining it in a muffle furnace at 500℃ for 3 hours with a heating rate of 4℃ / min.

[0050] ⑤ Dilute 10g of the binder polytetrafluoroethylene emulsion with 20g of deionized water and mix evenly to obtain a binder solution; weigh 30g of the catalyst sample, grind it to below 200 mesh, add it to the above binder solution, and stir continuously to form a slurry.

[0051] ⑥Immerse the honeycomb ceramic with a porosity of 50% and a pore size of 15μm into the slurry, and try to make the slurry evenly loaded on the carrier. After 5 minutes, take it out and dry it at 130℃ for later use. In this embodiment, the mass of CuMnCeOx catalyst loaded on the honeycomb ceramic is 15% of the mass of the honeycomb ceramic.

[0052] The low-ozone plasma generator prepared using this embodiment is placed in a 3m³ volume container. 2 In a sealed space, Staphylococcus aureus is introduced into the sealed space, the low ozone plasma generator in this embodiment is started, and an AC voltage of 15kV is applied to the needle plate electrode structure in the low ozone plasma generator for real-time discharge for 5 minutes.

[0053] The bacterial count in the air before and after the low-ozone plasma generator was tested. The Staphylococcus aureus kill rate was calculated using the formula: Staphylococcus aureus kill rate = (bacterial count in the air before operation - bacterial count in the air after operation) / bacterial count in the air before operation * 100%. The Staphylococcus aureus kill rate (%) was obtained, and the ozone content in the air after operation (ppm) was also measured. Simultaneously, the Staphylococcus aureus kill rate (%) and ozone content (ppm) were measured when only plasma generator 1 was used. The results are shown in Table 1 below.

[0054] Table 1

[0055] Staphylococcus aureus kill rate / % Ozone content / ppm Low ozone plasma generator 99.99% 0.3 Plasma generator 93.28% 25

[0056] As can be seen from the above data, the low-ozone plasma generator of this embodiment not only significantly reduces the ozone content to within a safe concentration range, but also significantly improves the sterilization efficiency of the plasma generator, with remarkable effects.

[0057] Example 2

[0058] A low-ozone plasma generator has the same structure as in Example 1, except that the honeycomb ceramic loaded with CuMnCeOx catalyst is different in this example. The preparation method of the honeycomb ceramic loaded with CuMnCeOx catalyst in this example is as follows:

[0059] ① Weigh out the Mn precursor, Ce precursor, and Cu precursor in a molar ratio of 5:2:1 and dissolve them in deionized water; wherein the Mn precursor is manganese nitrate, the Ce precursor is cerium nitrate, and the Cu precursor is copper sulfate.

[0060] ② Transfer the mixture to a hydrothermal reactor and react at 130°C for 12 hours;

[0061] ③ Wash and filter, then dry overnight at 100℃;

[0062] ④ The catalyst sample was obtained by calcining it in a muffle furnace at 500℃ for 3 hours with a heating rate of 4℃ / min.

[0063] ⑤ Dilute 10g of the PTFE emulsion binder with 20g of deionized water and mix evenly to obtain a binder solution; weigh 30g of catalyst powder, grind it to below 200 mesh, add it to the binder solution above, and stir continuously to form a slurry.

[0064] ⑥Immerse the honeycomb ceramic with a porosity of 50% and a pore size of 15μm, the same as in Example 1, into the slurry and try to make the slurry evenly loaded on the carrier. After 5 minutes, take it out and dry it at 130°C for later use.

[0065] The low-ozone plasma generator prepared using this embodiment is placed in a 3m³ volume container. 2 In a sealed space, Staphylococcus aureus is introduced into the sealed space, the low ozone plasma generator in this embodiment is started, and an AC voltage of 15kV is applied to the needle plate electrode structure in the low ozone plasma generator for real-time discharge for 5 minutes.

[0066] The bacterial count in the air before and after the low-ozone plasma generator was tested. The Staphylococcus aureus kill rate was calculated using the formula: Staphylococcus aureus kill rate = (bacterial count in the air before operation - bacterial count in the air after operation) / bacterial count in the air before operation * 100%. The Staphylococcus aureus kill rate (%) was obtained, and the ozone content in the air after operation (ppm) was also measured. Simultaneously, the Staphylococcus aureus kill rate (%) and ozone content (ppm) were measured when only plasma generator 1 was used. The results are shown in Table 2 below.

[0067] Table 2

[0068] Staphylococcus aureus kill rate / % Ozone content / ppm Low ozone plasma generator 98.97% 2.5 Plasma generator 93.28% 25

[0069] As can be seen from the above data, the low-ozone plasma generator of this embodiment not only significantly reduces the ozone content to within a safe concentration range, but also significantly improves the sterilization efficiency of the plasma generator, with remarkable effects.

[0070] Example 3

[0071] A low-ozone plasma generator has the same structure as in Example 1, except that the honeycomb ceramic loaded with CuMnCeOx catalyst is different in this example. The preparation method of the honeycomb ceramic loaded with CuMnCeOx catalyst in this example is as follows:

[0072] ① Weigh out the Mn precursor, Ce precursor, and Cu precursor in a molar ratio of 5:2:1 and dissolve them in deionized water; wherein the Mn precursor is manganese acetate, the Ce precursor is cerium oxide, and the Cu precursor is copper nitrate.

[0073] ② Transfer the mixture to a hydrothermal reactor and react at 130°C for 12 hours;

[0074] ③ Wash and filter, then dry overnight at 100℃;

[0075] ④ The catalyst sample was obtained by calcining it in a muffle furnace at 500℃ for 3 hours with a heating rate of 4℃ / min.

[0076] ⑤ Dilute 10g of the PTFE emulsion binder with 20g of deionized water and mix evenly to obtain a binder solution; weigh 30g of catalyst powder, grind it to below 200 mesh, add it to the binder solution above, and stir continuously to form a slurry.

[0077] ⑥Immerse the honeycomb ceramic with a porosity of 50% and a pore size of 15μm, the same as in Example 1, into the slurry and try to make the slurry evenly loaded on the carrier. After 5 minutes, take it out and dry it at 130°C for later use.

[0078] The low-ozone plasma generator prepared using this embodiment is placed in a 3m³ volume container. 2 In a sealed space, Staphylococcus aureus is introduced into the sealed space, the low ozone plasma generator in this embodiment is started, and an AC voltage of 15kV is applied to the needle plate electrode structure in the low ozone plasma generator for real-time discharge for 5 minutes.

[0079] The bacterial count in the air before and after the low-ozone plasma generator was tested. The Staphylococcus aureus kill rate was calculated using the formula: Staphylococcus aureus kill rate = (bacterial count in the air before operation - bacterial count in the air after operation) / bacterial count in the air before operation * 100%. The Staphylococcus aureus kill rate (%) was obtained, and the ozone content in the air after operation (ppm) was also measured. Simultaneously, the Staphylococcus aureus kill rate (%) and ozone content (ppm) were measured when only plasma generator 1 was used. The test results are shown in Table 3 below.

[0080] Table 3

[0081] Staphylococcus aureus kill rate / % Ozone content / ppm Low ozone plasma generator 99.36% 1.3 Plasma generator 93.28% 25

[0082] As can be seen from the above data, the low-ozone plasma generator of this embodiment not only significantly reduces the ozone content to within a safe concentration range, but also significantly improves the sterilization efficiency of the plasma generator, with remarkable effects.

[0083] Example 4

[0084] A low-ozone plasma generator has the same structure as in Example 1, except that the honeycomb ceramic loaded with CuMnCeOx catalyst is different in this example. The preparation method of the honeycomb ceramic loaded with CuMnCeOx catalyst in this example is as follows:

[0085] ① Weigh out the Mn precursor, Ce precursor, and Cu precursor in a molar ratio of 5:2:1 and dissolve them in deionized water; wherein the Mn precursor is potassium permanganate, the Ce precursor is cerium nitrate, and the Cu precursor is copper nitrate.

[0086] ② Transfer the mixture to a hydrothermal reactor and react at 100°C for 15 hours;

[0087] ③ Wash and filter, then dry overnight at 80℃;

[0088] ④ The catalyst sample was obtained by calcining it in a muffle furnace at 400℃ for 4 hours with a heating rate of 5℃ / min.

[0089] ⑤ Dilute 10g of the PTFE emulsion binder with 20g of deionized water and mix evenly to obtain a binder solution; weigh 30g of catalyst powder, grind it to below 200 mesh, add it to the binder solution above, and stir continuously to form a slurry.

[0090] ⑥Immerse the honeycomb ceramic with a porosity of 50% and a pore size of 15μm, the same as in Example 1, into the slurry and try to make the slurry evenly loaded on the carrier. After 5 minutes, take it out and dry it at 100°C for later use.

[0091] The low-ozone plasma generator prepared using this embodiment is placed in a 3m³ volume container. 2 In a sealed space, Staphylococcus aureus is introduced into the sealed space, the low ozone plasma generator in this embodiment is started, and an AC voltage of 15kV is applied to the needle plate electrode structure in the low ozone plasma generator for real-time discharge for 5 minutes.

[0092] The bacterial count in the air before and after the low-ozone plasma generator was tested. The Staphylococcus aureus kill rate was calculated using the formula: Staphylococcus aureus kill rate = (bacterial count in the air before operation - bacterial count in the air after operation) / bacterial count in the air before operation * 100%. The Staphylococcus aureus kill rate (%) was obtained, and the ozone content in the air after operation (ppm) was also measured. Simultaneously, the Staphylococcus aureus kill rate (%) and ozone content (ppm) were measured when only plasma generator 1 was used. The test results are shown in Table 4 below.

[0093] Table 4

[0094] Staphylococcus aureus kill rate / % Ozone content / ppm Low ozone plasma generator 98.56% 4.3 Plasma generator 93.28% 25

[0095] As can be seen from the above data, the low-ozone plasma generator of this embodiment not only significantly reduces the ozone content to within a safe concentration range, but also significantly improves the sterilization efficiency of the plasma generator, with remarkable effects.

[0096] Example 5

[0097] A low-ozone plasma generator has the same structure as in Example 1, except that the honeycomb ceramic loaded with CuMnCeOx catalyst is different in this example. The preparation method of the honeycomb ceramic loaded with CuMnCeOx catalyst in this example is as follows:

[0098] ① Weigh out the Mn precursor, Ce precursor, and Cu precursor in a molar ratio of 5:2:1 and dissolve them in deionized water; wherein the Mn precursor is potassium permanganate, the Ce precursor is cerium nitrate, and the Cu precursor is copper nitrate.

[0099] ② Transfer the mixture to a hydrothermal reactor and react at 150°C for 10 hours;

[0100] ③ Wash and filter, then dry overnight at 120℃;

[0101] ④ The catalyst sample was obtained by calcining at 600℃ for 2 hours in a muffle furnace at a heating rate of 2℃ / min.

[0102] ⑤ Dilute 10g of the PTFE emulsion binder with 20g of deionized water and mix evenly to obtain a binder solution; weigh 30g of catalyst powder, grind it to below 200 mesh, add it to the binder solution above, and stir continuously to form a slurry.

[0103] ⑥Immerse the honeycomb ceramic with a porosity of 50% and a pore size of 15μm, the same as in Example 1, into the slurry and try to make the slurry evenly loaded on the carrier. After 5 minutes, take it out and dry it at 150°C for later use.

[0104] The low-ozone plasma generator prepared using this embodiment is placed in a 3m³ volume container. 2 In a sealed space, Staphylococcus aureus is introduced into the sealed space, the low ozone plasma generator in this embodiment is started, and an AC voltage of 15kV is applied to the needle plate electrode structure in the low ozone plasma generator for real-time discharge for 5 minutes.

[0105] The bacterial count in the air before and after the low-ozone plasma generator was tested. The Staphylococcus aureus kill rate was calculated using the formula: Staphylococcus aureus kill rate = (bacterial count in the air before operation - bacterial count in the air after operation) / bacterial count in the air before operation * 100%. The Staphylococcus aureus kill rate (%) was obtained, and the ozone content in the air after operation (ppm) was also measured. Simultaneously, the Staphylococcus aureus kill rate (%) and ozone content (ppm) were measured when only plasma generator 1 was used. The results are shown in Table 5 below.

[0106] Table 5

[0107] Staphylococcus aureus kill rate / % Ozone content / ppm Low ozone plasma generator 98.95% 3.6 Plasma generator 93.28% 25

[0108] As can be seen from the above data, the low-ozone plasma generator of this embodiment not only significantly reduces the ozone content to within a safe concentration range, but also significantly improves the sterilization efficiency of the plasma generator, with remarkable effects.

[0109] Comparative Example 1

[0110] A plasma generating device with the same structure as in Example 1, except that the honeycomb ceramic loaded with CuMnCeOx catalyst in this comparative example is different. In this example, the honeycomb ceramic loaded with CuMnCeOx catalyst is directly replaced by the same honeycomb ceramic as in Example 1.

[0111] The plasma generator prepared using this comparative example was placed in a 3m³ volume container. 2 In a sealed space, Staphylococcus aureus is introduced into the sealed space, the plasma generator in this embodiment is started, and an AC voltage of 15kV is applied to the needle plate electrode structure in the plasma generator for real-time discharge for 5 minutes.

[0112] The bacterial count in the air before and after the plasma generator was operated was measured. The Staphylococcus aureus kill rate was calculated using the formula: Staphylococcus aureus kill rate = (bacterial count in the air before operation - bacterial count in the air after operation) / bacterial count in the air before operation * 100%. The Staphylococcus aureus kill rate (%) was obtained, and the ozone content in the air after operation (ppm) was also measured. Simultaneously, the Staphylococcus aureus kill rate (%) and ozone content (ppm) were measured when only plasma generator 1 was used. The results are shown in Table 6 below.

[0113] Table 6

[0114]

[0115] The data above shows that the plasma generator with honeycomb ceramics in this comparative example not only failed to reduce ozone content, but even slightly increased it. Moreover, the sterilization effect was less than ideal after the ozone content was slightly increased.

[0116] Comparative Example 2

[0117] A low-ozone plasma generator has the same structure as in Example 1, except that the honeycomb ceramic loaded with CuMnCeOx catalyst in this comparative example is different. In this comparative example, the honeycomb ceramic loaded with CuMnCeOx catalyst is replaced with activated carbon of the same volume. The specific preparation method is as follows:

[0118] ① Weigh out the Mn precursor, Ce precursor, and Cu precursor in a molar ratio of 5:2:1 and dissolve them in deionized water; wherein the Mn precursor is potassium permanganate, the Ce precursor is cerium nitrate, and the Cu precursor is copper nitrate.

[0119] ② Transfer the mixture to a hydrothermal reactor and react at 130°C for 12 hours;

[0120] ③ Wash and filter, then dry overnight at 100℃;

[0121] ④ The catalyst sample was obtained by calcining it in a muffle furnace at 500℃ for 3 hours with a heating rate of 4℃ / min.

[0122] ⑤ Dilute 10g of the PTFE emulsion binder with 20g of deionized water and mix evenly to obtain a binder solution; weigh 30g of catalyst powder, grind it to below 200 mesh, add it to the binder solution above, and stir continuously to form a slurry.

[0123] ⑥Immerse activated carbon blocks of the same volume as the honeycomb ceramic in Example 1 into the slurry, and try to make the slurry evenly loaded on the carrier. After 5 minutes, take them out and dry them at 130°C for later use. The loading amount in this comparative example is basically equivalent to that in Example 1.

[0124] The low-ozone plasma generator prepared using this embodiment is placed in a 3m³ volume container. 2 In a sealed space, Staphylococcus aureus is introduced into the sealed space, the low ozone plasma generator in this embodiment is started, and an AC voltage of 15kV is applied to the needle plate electrode structure in the low ozone plasma generator for real-time discharge for 5 minutes.

[0125] The bacterial count in the air before and after the low-ozone plasma generator was tested. The Staphylococcus aureus kill rate was calculated using the formula: Staphylococcus aureus kill rate = (bacterial count in the air before operation - bacterial count in the air after operation) / bacterial count in the air before operation * 100%. The Staphylococcus aureus kill rate (%) was obtained, and the ozone content in the air after operation (ppm) was also measured. Simultaneously, the Staphylococcus aureus kill rate (%) and ozone content (ppm) were measured when only plasma generator 1 was used. The test results are shown in Table 7 below.

[0126] Table 7

[0127] Staphylococcus aureus kill rate / % Ozone content / ppm Low ozone plasma generator 94.26% 21.5 Plasma generator 93.28% 25

[0128] As can be seen from the above data, the low-ozone plasma generator in this embodiment can slightly reduce the ozone content and improve the sterilization rate, but its ozone content is still high, exceeding the safe concentration range.

[0129] Comparative Example 3

[0130] A low-ozone plasma generator has the same structure as in Example 1, except that the honeycomb ceramic loaded with CuMnCeOx catalyst in this comparative example is different. The preparation method of the honeycomb ceramic loaded with CuMnCeOx catalyst in this comparative example is as follows:

[0131] ① Weigh out the Mn precursor, Ce precursor, and Cu precursor in a molar ratio of 3:2:1 and dissolve them in deionized water; wherein the Mn precursor is potassium permanganate, the Ce precursor is cerium nitrate, and the Cu precursor is copper nitrate.

[0132] ② Transfer the mixture to a hydrothermal reactor and react at 130°C for 12 hours;

[0133] ③ Wash and filter, then dry overnight at 100℃;

[0134] ④ The catalyst sample was obtained by calcining it in a muffle furnace at 500℃ for 3 hours with a heating rate of 4℃ / min.

[0135] ⑤ Dilute 10g of the PTFE emulsion binder with 20g of deionized water and mix evenly to obtain a binder solution; weigh 30g of catalyst powder, grind it to below 200 mesh, add it to the binder solution above, and stir continuously to form a slurry.

[0136] ⑥Immerse the honeycomb ceramic with a porosity of 50% and a pore size of 15μm, the same as in Example 1, into the slurry and try to make the slurry evenly loaded on the carrier. After 5 minutes, take it out and dry it at 130°C for later use.

[0137] The low-ozone plasma generator prepared using this embodiment is placed in a 3m³ volume container. 2 In a sealed space, Staphylococcus aureus is introduced into the sealed space, the low ozone plasma generator in this embodiment is started, and an AC voltage of 15kV is applied to the needle plate electrode structure in the low ozone plasma generator for real-time discharge for 5 minutes.

[0138] The bacterial count in the air before and after the low-ozone plasma generator was tested. The Staphylococcus aureus kill rate was calculated using the formula: Staphylococcus aureus kill rate = (bacterial count in the air before operation - bacterial count in the air after operation) / bacterial count in the air before operation * 100%. The Staphylococcus aureus kill rate (%) was obtained, and the ozone content in the air after operation (ppm) was also measured. Simultaneously, the Staphylococcus aureus kill rate (%) and ozone content (ppm) were measured when only plasma generator 1 was used. The results are shown in Table 8 below.

[0139] Table 8

[0140]

[0141]

[0142] The data above shows that the CuMnCeOx catalyst in this comparative example, when used in excess of the specified proportion, cannot achieve a high sterilization rate and a low ozone concentration.

[0143] The present invention also verified that the loading of CuMnCeOx catalyst in the honeycomb ceramic is 10-20 wt.%. The lower the loading, the ozone content per unit time gradually increases and the sterilization efficiency gradually decreases. However, within this range, the requirements for good sterilization effect and ozone safety concentration can be met. The higher the loading, the less significant the reduction of ozone content and the improvement of sterilization efficiency. In the present invention, the preferred loading of CuMnCeOx catalyst in the honeycomb ceramic is 10-20 wt.%, and more preferably 15 wt.%.

[0144] Similarly, the mass ratio between CuMnCeOx catalyst and binder was also studied. Within the range of (2.5-3.5):1, the requirement for stable adhesion of CuMnCeOx catalyst on honeycomb ceramics was met, ensuring good sterilization effect and ozone safety concentration requirements.

[0145] Meanwhile, verification showed that honeycomb ceramics with a porosity of 40-60% and a pore size of 10-20 μm, when applied to this invention to prepare a catalytic structure for reducing ozone levels in plasma generators, can also reduce ozone concentration to a safe range when applied to plasma generators, while maintaining or even improving the sterilization rate of the plasma generator. Therefore, the catalytic structure composed of honeycomb ceramics with a porosity of 40-60% and a pore size of 10-20 μm, when applied to plasma generators, can meet the requirements of ensuring good sterilization effect and safe ozone concentration.

[0146] Furthermore, this invention also verified that applying an AC voltage of 11 kV to the needle-plate electrode structure in the low-ozone plasma generator achieves essentially the same effect as this invention under this voltage condition. This demonstrates that the low-ozone plasma generator of this invention can meet the requirements of this invention within an AC voltage range of 11-15 kV.

[0147] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. An application of a low-ozone plasma generator in converting ozone into highly oxidizing superoxide radicals, characterized in that, The low-ozone plasma generator includes a plasma generator (1) for generating ozone, and a honeycomb ceramic loaded with a CuMnCeOx catalyst disposed in the plasma generation region of the plasma generator (1); the molar ratio of Mn, Ce and Cu in the CuMnCeOx catalyst is 5:2:

1. The porosity of the honeycomb ceramic is 40%-60%, and the pore size of the honeycomb ceramic is 10-20μm; The loading of CuMnCeOx catalyst in the honeycomb ceramic is 10%-20%.

2. The application according to claim 1, characterized in that, The loading of CuMnCeOx catalyst in the honeycomb ceramic is 15%.

3. The application according to any one of claims 1-2, characterized in that, The method for preparing the honeycomb ceramic supported on CuMnCeOx catalyst includes: Precursor salts of Mn, Ce, and Cu were obtained and dissolved in deionized water to obtain a precursor mixture. The precursor mixture was subjected to a hydrothermal reaction. After the hydrothermal reaction is complete, wash, filter, and perform the first drying. The CuMnCeOx catalyst was obtained by calcination after the first drying. The CuMnCeOx catalyst was ground to below 200 mesh and added to the binder solution to form a slurry; The honeycomb ceramic is mixed with a slurry to allow the slurry to adhere to the honeycomb ceramic. After a second drying, a honeycomb ceramic loaded with a CuMnCeOx catalyst is obtained.

4. The application according to claim 3, characterized in that, The hydrothermal reaction is carried out at a temperature of 100-150 °C for 10-15 h. And / or, the first drying method is: overnight drying at 80 ℃~120 ℃; And / or, the calcination temperature is 400 ℃~600 ℃, the calcination time is 2~4 h, and the heating rate is 2~5 ℃ / min; And / or, the honeycomb ceramic is impregnated in a slurry to allow the slurry to adhere; And / or, the temperature for the second drying is 100~150℃.

5. The application according to claim 4, characterized in that, The soaking time should be at least 5 minutes.

6. The application according to claim 1, characterized in that, The plasma generating device (1) is a needle-plate electrode structure with dielectric barrier discharge.

Citation Information

Patent Citations

  • Plasma sterilization and disinfection cabinet and disinfection method

    CN112294991A

  • Plasma sterilization process, device and equipment

    CN117357673A

  • Plasma air disinfection device and method for in-situ inhibition and elimination of ozone

    CN112604495A

  • Microorganism disinfecting and killing device based on synergy of plasma and catalytic technology

    CN115737860A