Method for removing the edge-pulling machine online during the forming process of Mini LED back panel glass
By precisely adjusting the speed and angle of the edge-pulling machine, the impact of oxide accumulation on product quality during float glass production was resolved, ensuring the stability and efficiency of the production process and reducing quality losses due to improper maintenance and operation.
Patent Information
- Application Number
- CN202410637674.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-22
- Publication Date
- 2026-11-24
- Estimated Expiration
- 2044-05-22
AI Technical Summary
In the float glass production process, the accumulation of oxides generated by the edge-pulling machine in the tin bath under high temperature conditions can affect the quality of glass products. Moreover, the existing technology lacks a systematic method for removing the edge-pulling machine, resulting in unstable production efficiency and product quality.
By precisely adjusting the speed and angle of the edge-pulling machine, the pulling speed of the glass strip is gradually reduced. The angle of the edge-pulling machine is adjusted and the edge-pulling wheel is lifted to remove it from the molten glass, ensuring that the impact on glass production is minimized during the removal process.
This reduces the impact on glass production during the maintenance of the edge-pulling machine, improves production efficiency, ensures product quality stability, and reduces product quality losses caused by improper maintenance operations.
Smart Images

Figure CN118598477B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of glass production technology, specifically to a method for online removal of the edge-pulling machine during the forming process of Mini LED backplate glass. Background Technology
[0002] In the float glass production process, the tin bath edge-drawing machine plays a crucial role, controlling the width and thickness of the glass. During float glass forming, the tin bath continuously generates gaseous oxides under high temperatures. These oxides gradually accumulate on the surface of the edge-drawing machine's head and rod, forming a solid oxide layer upon cooling. As the oxides accumulate, they may detach and fall into the tin bath under gravity or vibration, affecting the quality of the glass product. Therefore, to prevent the oxides from adversely affecting the glass product, when the oxides on the edge-drawing machine reach a certain level, it is essential to remove the machine from the tin bath promptly and thoroughly clean and maintain it. This process is crucial for ensuring the smooth operation of the glass production process and the stability of product quality.
[0003] During the maintenance of the edge-pulling machine, in order to ensure the continuity of the production process and the stability of product quality, the operating parameters of other edge-pulling machines must be appropriately adjusted. These adjustments must be precise, as any improper adjustments may negatively affect the dimensions and quality of the glass. Therefore, to improve production efficiency and product quality, a systematic method for adjusting the edge-pulling machine parameters to facilitate its removal is needed, ensuring the stability of the glass production process and the consistency of product quality during the removal process. Summary of the Invention
[0004] The technical problem to be solved by this invention is to overcome the shortcomings of the prior art and provide a method for online removal of the edge-pulling machine during the forming process of Mini LED backplate glass. It systematically proposes a solution to the problem of removing the edge-pulling machine used in the production of tin bath during float glass forming. By precisely adjusting the parameters during the removal process of the edge-pulling machine, not only is the production efficiency improved, but the stability of product quality is also ensured.
[0005] The technical solution of this invention is as follows:
[0006] Method for removing the edge-pulling machine online during the forming process of Mini LED back panel glass:
[0007] (1) Method for removing the No. 1 edge-pulling machine
[0008] 1) Reduce the main drive pulling speed of the glass belt
[0009] 2) Reduce the speed of edge pulling machines #2 and #3. After the smooth edge becomes larger, adjust the angle of edge pulling machine #1 from a positive angle to a negative angle, and increase the angle of edge pulling machines #2 and #3.
[0010] 3) Raise the No. 1 edge-pulling machine upward by 1 / 2 height so that its edge-pulling wheel is away from the molten glass. If no accident occurs after observation, raise the No. 1 edge-pulling machine to a horizontal position and then remove it.
[0011] (2) Method for removing the edge-pulling machine in the middle position
[0012] A) Reduce the pulling speed of the glass ribbon;
[0013] B) Reduce the speed of the next pair of edge-pulling machines at the middle position. After the smooth edge becomes larger, adjust the angle of the edge-pulling machine at the middle position from a positive angle to a negative angle, and increase the angle of edge-pulling machines #1 and #2.
[0014] C) Raise the middle edge-pulling machine upward by 1 / 2 height so that its edge-pulling wheel leaves the molten glass. If no accident occurs after observation, raise the middle edge-pulling machine to a horizontal position and then remove it.
[0015] (3) Method for removing the edge-pulling machine
[0016] a) Reduce the pulling speed of the glass ribbon;
[0017] b) Adjust the angle of the last pair of edge-pulling machines from a positive angle to a negative angle, increase the angle of the pair of edge-pulling machines in front of it, and increase the speed of the three pairs of edge-pulling machines in front of it.
[0018] c) Lift the last pair of edge-pulling machines to a horizontal position and then move them out.
[0019] The speed of the edge-pulling machine is the rotational speed of the edge-pulling wheel; the angle of the edge-pulling machine is the angle between the edge-pulling wheel and the central axis of the tin bath along its length.
[0020] Preferably, in step 1), the pulling speed of the glass ribbon is reduced to: V 末 =V 初 ×H 初 / H 末 H 末 =H 初 +0.1m, H 初 =K×D; where V 末 - Adjusted pulling speed, m / h; V 初 - Pulling speed before adjustment, m / h; H 初 -Empirical correction value for thickness before adjustment, in meters (m); H 末 - Adjusted empirical correction value for thickness, m; D - Glass strip thickness, mm; K = 2.24 m / mm.
[0021] Preferably, in step 2) (B), the light edge increases by 60±10mm.
[0022] Preferably, in step 2), the speed of edge pulling machine #2 is reduced by 3-7 m / h, and the speed of edge pulling machine #3 is reduced by 2-6 m / h; the angle of edge pulling machines #2 and #3 is increased to 15°.
[0023] Preferably, in step A), the pulling speed of the glass ribbon is reduced to: V 末 =V 初 ×H 初 / H 末 H 末 =H 初 +0.05m, H 初 =K×D; where V 末 - Adjusted pulling speed, m / h; V 初 - Pulling speed before adjustment, m / h; H 初 -Empirical correction value for thickness before adjustment, in meters (m); H 末 - Adjusted empirical correction value for thickness, m; D - Glass strip thickness, mm; K = 2.24 m / mm.
[0024] Preferably, in step B), the speed of the next pair of edge-pulling machines of the middle position edge-pulling machine is reduced to 5-8 m / h higher than the original speed of the middle position edge-pulling machine.
[0025] Preferably, in step a), the pulling speed of the glass ribbon is reduced to: V 末 =V 初 ×H 初 / H 末 H 末 =H 初 +0.05m, H 初 =K×D; where V 末 - Adjusted pulling speed, m / h; V 初 - Pulling speed before adjustment, m / h; H 初 -Empirical correction value for thickness before adjustment, in meters (m); H 末 - Adjusted empirical correction value for thickness, m; D - Glass strip thickness, mm; K = 2.24 m / mm.
[0026] Preferably, in step b), the angle of the pair of edge pulling machines before the last pair of edge pulling machines is increased by 6-8° and the speed is increased by 15-19 m / h, the speed of the second pair of edge pulling machines before the last pair of edge pulling machines is increased by 14-18 m / h, and the speed of the third pair of edge pulling machines before the last pair of edge pulling machines is increased by 12-16 m / h.
[0027] Compared with the prior art, the present invention has the following advantages:
[0028] 1. This invention systematically proposes a solution to the problem of removing the edge-pulling machine used in the tin bath production process of float glass. It allows for the adjustment of different process parameters according to the specific needs of different edge-pulling machines during maintenance. Through this precise adjustment, this invention effectively reduces the impact on glass production during edge-pulling machine maintenance and minimizes product quality losses caused by improper maintenance operations. By precisely adjusting parameters during the edge-pulling machine removal process, this invention not only improves production efficiency but also ensures the stability of product quality. Attached Figure Description
[0029] Figure 1 This is a schematic diagram of the tin bath with 12 pairs of edge-pulling machines in embodiments 1-3 of the present invention.
[0030] Figure 2 This is a schematic diagram showing the edge-pulling machine in the present invention in positive and negative angle states. The edge-pulling machine on the left is in the positive angle state, and the edge-pulling machine on the right is in the negative angle state.
[0031] In the diagram: 1. Tin bath; 2. No. 1 edge pulling machine; 3. No. 3 edge pulling machine; 4. No. 12 edge pulling machine; 5. Edge pulling wheel; 6. Polished edge; 7. Tooth mark. Detailed Implementation
[0032] To enable those skilled in the art to better understand the technical solutions of this invention, the technical solutions of this invention will be clearly and completely described below in conjunction with the embodiments of this invention.
[0033] like Figure 1 As shown in the following embodiments, the technical solution of the present invention is described using a solder bath 1 equipped with 12 pairs of edge-pulling machines as an example. The pair of edge-pulling machines closest to the inlet of the solder bath 1 is the first pair, namely edge-pulling machine 1# 2; the pair of edge-pulling machines closest to the outlet of the solder bath 1 is the last pair, namely edge-pulling machine 12# 4; and the rest are edge-pulling machines in intermediate positions, numbered sequentially from inlet to outlet as 2#, 3#...11#. The initial angle and speed of the 12 pairs of edge-pulling machines during normal operation are shown in Table 1:
[0034] Table 1.12 Initial Angles and Speeds of the Edge-Pulling Machine During Normal Operation
[0035]
[0036]
[0037] When cleaning 12 pairs of edge-pulling machines, the machines need to be removed first, cleaned, and then returned to their original positions. The following describes three scenarios for removing the edge-pulling machines from different locations.
[0038] Example 1
[0039] This embodiment provides a method for removing the #1 edge-pulling machine 2, including the following steps:
[0040] 1) The pulling speed of the 0.7mm thick glass strip was reduced from 500m / h to 470m / h. After each 5m / h reduction, the glass was observed for 5 minutes. This is because after each speed reduction, the temperature changes due to the slower movement of the glass, which will affect the shrinkage rate and may cause the edge to detach from the edge of the glass strip. Therefore, the observation time is also the time for the glass strip to stabilize. If this is done continuously, it will cause significant changes in the glass and lead to unstable quality.
[0041] 2) Gradually reduce the speed of edge-pulling machine #2 from 30m / h to 26m / h, and gradually reduce the speed of edge-pulling machine #3 from 37m / h to 33m / h. After the smooth edge (i.e., the glass edge) 6 increases in size (i.e., the glass edge expands outward) by 60mm, adjust the angle of edge-pulling machine #1 from 5° to -6° (e.g., ...). Figure 2 As shown), the angles of edge pulling machines #2 and #3 were increased to 15°. Except for the last adjustment, the adjustment increment was 0.3° each time. Each adjustment was performed by first adjusting edge pulling machine #1, followed by adjusting edge pulling machines #2 and #3. The angle adjustment increment was set to 0.3° each time because if the increment was too large, the glass would change significantly, which could lead to a large change in the width of the plate. If the increment was too small, it would result in too many adjustments and a longer operation time.
[0042] 3) Raise the No. 1 edge-pulling machine 2 by half its height so that its edge-pulling wheel 5 is away from the molten glass. Observe for about 1 minute. If no accident occurs, raise the No. 1 edge-pulling machine 2 to a horizontal position and remove it. After raising the No. 1 edge-pulling machine 2, pay special attention to the No. 2 edge-pulling machine to ensure that the distance between its tooth mark 7 (i.e. the mark produced where the edge-pulling wheel 5 of the edge-pulling machine contacts the molten glass) and the edge of the molten glass is within the normal range. This is to prevent the edge of the molten glass from contracting at this point after the No. 1 edge-pulling machine 2 is removed, which would cause the edge-pulling wheel 5 of the adjacent No. 2 edge-pulling machine to be forced to detach from the molten glass.
[0043] After lifting edge-pulling machine #1, clean the edge-pulling machines. After cleaning, restore each edge-pulling machine to its initial state.
[0044] Example 2
[0045] This embodiment provides a method for removing the middle-position edge-pulling machine (taking edge-pulling machine #3 as an example), including the following steps:
[0046] A) Reduce the pulling speed of the 0.7mm thick glass strip from 500m / h to 485m / h, and observe for 5min after each 5m / h reduction;
[0047] B) Gradually reduce the speed of the #4 edge-pulling machine to 42m / h. After the smooth edge 6 increases by 60mm, adjust the angle of the #3 edge-pulling machine to -6° (e.g., Figure 2 As shown), the angle of edge pulling machine 1 (2) is adjusted to 10° and the angle of edge pulling machine 2 (3) is adjusted to 15°. The adjustment range is 0.5° each time. When adjusting, edge pulling machines 1 and 2 are adjusted first, and then edge pulling machine 3 (3) is adjusted.
[0048] C) Raise the #3 edge-pulling machine 3 by half its height so that its edge-pulling wheel 5 is away from the molten glass. Observe for about 1 minute. If no accident occurs, raise the #3 edge-pulling machine 3 to a horizontal position and remove it. After raising the #3 edge-pulling machine 3, focus on adjusting the #1 edge-pulling machine 2 and the #2 edge-pulling machine, and observe to ensure that the distance between their tooth marks 7 and the edge of the molten glass is within the normal range.
[0049] After lifting edge-pulling machine #3, clean the edge-pulling machine. After cleaning, restore all edge-pulling machines to their initial state.
[0050] Example 3
[0051] This embodiment provides a method for removing the 12# edge-pulling machine 4, including the following steps:
[0052] a) Reduce the pulling speed of the 0.7mm thick glass strip from 500m / h to 485m / h, and observe for 5min after each 5m / h reduction;
[0053] b) Adjust the angle of edge pulling machine 4 (#12) to -5° and the angle of edge pulling machine 2 (#11) to 13°, with each adjustment increment being 0.5°. Each adjustment should be made by first adjusting edge pulling machine 4 (#12) and then adjusting edge pulling machine 2 (#11). Increase the speed of edge pulling machine 2 (#11) to 200 m / h, the speed of edge pulling machine 10 (#10) to 172 m / h, and the speed of edge pulling machine 9 (#9) to 146 m / h.
[0054] c) Lift the #12 edge-pulling machine 4 to a horizontal position and then remove it; after lifting the #12 edge-pulling machine 4, focus on adjusting the #1 edge-pulling machine 2 and the #11 edge-pulling machine 2, and observe to ensure that the distance between the tooth mark 7 and the edge of the glass melt is within the normal range.
[0055] After lifting edge-pulling machine #12, clean the edge-pulling machine. After cleaning, return each edge-pulling machine to its initial state.
[0056] This invention systematically proposes a solution to the problem of removing the edge-pulling machine used in the tin bath 1 during float glass production. It allows for the adjustment of different process parameters according to the specific needs of different edge-pulling machines during maintenance. Using this method, the glass thickness can be maintained within the range of 0.7±0.1mm, and the operation time can be effectively reduced from 2-3 hours per operation to 1 hour. Through this precise adjustment, this invention effectively reduces the impact on glass production during edge-pulling machine maintenance, minimizing product quality losses caused by improper maintenance operations. By precisely adjusting parameters during the edge-pulling machine removal process, this invention not only improves production efficiency but also ensures the stability of product quality.
Claims
1. A method for online removal of the edge-pulling machine during the forming process of Mini LED backplate glass, characterized in that, Method for removing the #1 edge-pulling machine: 1) Reduce the pulling speed of the glass ribbon; the pulling speed of the glass ribbon is reduced to: V 末 =V 初 ×H 初 / H 末 H 末 =H 初 +0.1m, H 初 =K×D; where V is the value of K×D. 末 - Adjusted pulling speed, m / h; V 初 - Pulling speed before adjustment, m / h; H 初 -Empirical correction value for thickness before adjustment, in meters (m); H 末 - Adjusted empirical correction value for thickness, m; D - Glass strip thickness, mm; K = 2.24 m / mm; 2) Reduce the speed of edge pulling machines #2 and #3. After the smooth edge (6) becomes larger, adjust the angle of edge pulling machine #1 from a positive angle to a negative angle, and increase the angle of edge pulling machines #2 and #3. Reduce the speed of edge pulling machine #2 by 3-7 m / h and the speed of edge pulling machine #3 by 2-6 m / h. Increase the angle of edge pulling machines #2 and #3 to 15°. 3) Raise the No. 1 edge-pulling machine by 1 / 2 height so that its edge-pulling wheel (5) leaves the glass liquid. If no accident occurs after observation, raise the No. 1 edge-pulling machine to a horizontal state and then move it out.
2. A method for online removal of the edge-pulling machine during the forming process of Mini LED backplate glass, characterized in that, Method for removing the edge-pulling machine in the middle position: A) Reduce the pulling speed of the glass ribbon; the pulling speed of the glass ribbon is reduced to: V 末 =V 初 ×H 初 / H 末 H 末 =H 初 +0.05m, H 初 =K×D; where V is the value of K×D. 末 - Adjusted pulling speed, m / h; V 初 - Pulling speed before adjustment, m / h; H 初 -Empirical correction value for thickness before adjustment, in meters (m); H 末 - Adjusted empirical correction value for thickness, m; D - Glass strip thickness, mm; K = 2.24 m / mm; B) Reduce the speed of the next pair of edge-pulling machines of the middle edge-pulling machine. After the smooth edge (6) becomes larger, adjust the angle of the middle edge-pulling machine from a positive angle to a negative angle, and increase the angle of edge-pulling machines 1 and 2. Reduce the speed of the next pair of edge-pulling machines of the middle edge-pulling machine to 5-8 m / h higher than the original speed of the middle edge-pulling machine. C) Raise the middle edge-pulling machine upward by 1 / 2 height so that its edge-pulling wheel (5) leaves the glass liquid. If no accident occurs after observation, raise the middle edge-pulling machine to a horizontal state and then move it out.
3. A method for online removal of the edge-pulling machine during the forming process of Mini LED backplate glass, characterized in that, Method for removing the edge-pulling machine: a) Reduce the pulling speed of the glass ribbon; the pulling speed of the glass ribbon is reduced to: V 末 =V 初 ×H 初 / H 末 H 末 =H 初 +0.05m, H 初 =K×D; where V is the value of K×D. 末 - Adjusted pulling speed, m / h; V 初 - Pulling speed before adjustment, m / h; H 初 -Empirical correction value for thickness before adjustment, in meters (m); H 末 - Adjusted empirical correction value for thickness, m; D - Glass strip thickness, mm; K = 2.24 m / mm; b) Adjust the angle of the last pair of edge-pulling machines from a positive angle to a negative angle, increase the angle of the pair of edge-pulling machines in front of it, and increase the speed of the three pairs of edge-pulling machines in front of it; increase the angle of the pair of edge-pulling machines in front of the last pair of edge-pulling machines by 6-8° and increase the speed by 15-19m / h, increase the speed of the second pair of edge-pulling machines in front of the last pair of edge-pulling machines by 14-18m / h, and increase the speed of the third pair of edge-pulling machines in front of the last pair of edge-pulling machines by 12-16m / h; c) Lift the last pair of edge-pulling machines to a horizontal position and then move them out.
Citation Information
Patent Citations
Hanging type edge roller for producing float glass
CN105417936A
Method for producing float glass with front rotation point projection and meshing point coincided
CN106045281A