Preparation and construction process of copper tailing slag road material
By using copper tailings slag and low-carbon gel materials to prepare new road materials, the problems of cumbersome and high-cost construction of traditional cement-stabilized crushed stone have been solved, realizing the application of efficient, low-carbon and environmentally friendly road materials, shortening the construction period and reducing costs.
Patent Information
- Application Number
- CN202410540218.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-30
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-04-30
AI Technical Summary
In traditional road design, the use of cement-stabilized crushed stone materials for the road base layer leads to complicated construction, long construction period, high cost, and strong resource dependence, requiring a more efficient and low-carbon material alternative.
A novel road material is prepared by using copper tailings slag and low-carbon gel material. The copper tailings slag accounts for 92-97 wt%, and the low-carbon gel material accounts for 3-8 wt%. The copper tailings slag and the mixed low-carbon gel material are processed through a specific process to form a material suitable for road engineering.
The material's 3-day unconfined compressive strength is comparable to that of traditional cement-stabilized crushed stone after 7 days, shortening the construction period by 4 days, reducing material costs by 78%, reducing carbon dioxide emissions, protecting the ecological environment, and reducing tailings dam risks.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This application relates to the field of road engineering technology, and in particular to a preparation and construction process for copper tailings slag road materials. Background Technology
[0002] Traditional road design proceeds from bottom to top as follows: embankment, subgrade, and pavement structure. Cement-stabilized crushed stone is typically used for the pavement base layer. This material involves a variety of aggregate types and relies heavily on cement for binding, making the compaction process cumbersome. It often requires 7 days of core sampling to verify strength before proceeding to the next stage, impacting construction time and increasing overall costs. Given this context, utilizing copper tailings to replace traditional sand and gravel, and using solid waste-based low-carbon cementitious materials to replace silicate cement, are key challenges that need to be addressed. This includes reducing road construction cycles and using copper tailings slag and cementitious materials to collaboratively prepare novel road materials. Summary of the Invention
[0003] In order to solve at least one of the above-mentioned technical problems and develop a high-performance copper tailings slag road material, this application provides a copper tailings slag road material preparation and construction process.
[0004] On the one hand, this application provides a copper tailings slag-based road material, comprising 92-97 wt% copper tailings slag and 3-8 wt% low-carbon gel material;
[0005] The copper tailings slag contains a total content of CaO, SiO2, Al2O3, and MgO compounds ≥70%, a moisture content ≤14%, a loss on ignition ≤20%, and an SO3 content ≤3.0%.
[0006] The low-carbon gel material comprises 80-85 wt% slag powder and steel slag powder, 8-12 wt% gypsum powder, 6.5-10.5 wt% alkaline activating material, and 0.5-0.8 wt% additives.
[0007] Optionally, the copper tailings residue on a 200-mesh sieve is ≥40%, and the moisture content is ≤14%.
[0008] Optionally, the alkaline activating material is a mixture of sodium metasilicate, sodium silicate, and carbide slag in a ratio of 1:1:8.
[0009] Optionally, the additive may be either potassium aluminum sulfate or sodium thiosulfate.
[0010] Optionally, the moisture content of the copper tailings road material is 8-12 wt%.
[0011] Secondly, this application provides a method for preparing the aforementioned copper tailings slag-based road material, comprising the following steps:
[0012] S1, Preparation of low-carbon gel materials
[0013] Mix slag powder and steel slag powder in a 4:1 ratio, then add gypsum powder, alkaline activating material and additives, and mix evenly.
[0014] S2, Copper Tailings Preparation
[0015] The copper tailings slag is graded and dewatered through a sandblasting screen and a ceramic filter to control the copper tailings slag residue on a 200-mesh screen to be ≥40% and the moisture content to be ≤14%.
[0016] S3, Preparation of Road Materials from Copper Tailings Slag
[0017] The low-carbon gel material prepared in S1 was incorporated into the copper tailings slag prepared in S2 in a certain proportion, and the dosage of the gel material was detected by EDTA titration experiment. The dosage was controlled at 3-8 ± 0.2 wt%, and the overall moisture content was 8-12 wt%.
[0018] S4. The copper tailings slag road material prepared in S3 is paved, compacted, and cured. The paving thickness is controlled to be ≤300mm; the slurry coefficient is controlled to be 1.6~1.8; two passes with a vibratory roller and two passes with a single / double steel drum roller, and the compaction degree is controlled to be ≥93%; curing is carried out by watering or natural rainwater; and core sampling is performed after 3 days.
[0019] Thirdly, this application provides the application of the aforementioned copper tailings slag-based road materials in the field of road engineering.
[0020] In summary, the present invention has at least one of the following beneficial technical effects:
[0021] By using copper tailings to replace traditional sand and gravel, and by using solid waste-based low-carbon cementitious materials to replace cement, material costs are reduced. This application designs the ratio of copper tailings slag to low-carbon cementitious materials and selects superior copper tailings slag and compatible low-carbon cementitious materials. The 3-day unconfined compressive strength of this material is comparable to the 7-day strength of traditional cement-stabilized crushed stone. Subsequent construction processes can be completed 4 days earlier than with cement-stabilized crushed stone materials, significantly shortening the construction period.
[0022] 1. Carbon Reduction Benefits: Replacing cement with solid waste-based cementitious materials results in carbon dioxide emissions of 616.6 kg per ton of cement production and processing. Solid waste-based low-carbon cementitious materials mainly involve the mixing of powder materials, with a power consumption of 7.5 kWh per ton of processing. Referring to the General Rules for Comprehensive Energy Consumption Calculation in GB / T 2589-2020, the carbon dioxide emissions per ton of new low-carbon cementitious materials can be calculated to be 2.24 kg. The use of each ton of solid waste-based cementitious materials can effectively reduce regional carbon dioxide emissions by 614.36 kg; the application of each ton of copper tailings slag road materials can effectively reduce regional carbon dioxide emissions by 18.43–49.14 kg.
[0023] 2. Environmental benefits: After the tailings are backfilled, the excess portion is mainly discharged into the tailings pond. The high-volume use of copper tailings slag can effectively reduce the amount of tailings discharged into the tailings pond, thereby reducing the safety and environmental risks of the tailings pond. At the same time, copper tailings effectively replace natural resources such as sand and gravel, protecting the ecological environment.
[0024] 3. Construction benefits: Copper tailings slag road material has a thicker paving thickness, avoiding secondary paving. At the same time, it has more construction tools to choose from during the compaction process, reduces the number of passes, and eliminates the need for final compaction. Compared with traditional cement-stabilized crushed stone, it greatly improves construction efficiency. Most importantly, its 3-day unconfined compressive strength is comparable to the 7-day strength of traditional cement-stabilized crushed stone. Subsequent construction processes can be completed 4 days earlier than with cement-stabilized crushed stone, greatly shortening the construction period.
[0025] 4. Economic Benefits: Copper tailings slag road materials are made primarily from tailings, are easy to process, require less equipment investment, and have a comprehensive ex-factory cost of approximately 55 yuan / ton. The same amount of stabilized crushed stone currently costs approximately 98 yuan / ton. Copper tailings slag road materials reduce costs by 78% compared to traditional cement-stabilized crushed stone. At the same time, the current cost of discharging tailings into tailings ponds is approximately 30 yuan / ton. Using copper tailings to prepare road materials for road engineering can directly reduce the cost of mine tailings discharge, which is conducive to the sustainable operation of mines and the healthy development of the regional economy. Detailed Implementation
[0026] The present application will be further described in detail below with reference to the embodiments.
[0027] This application designs a copper tailings slag-based road material, comprising 92-97 wt% copper tailings slag and 3-8 wt% low-carbon gel material;
[0028] The copper tailings slag contains a total content of CaO, SiO2, Al2O3, and MgO compounds ≥70%, a moisture content ≤14%, a loss on ignition ≤20%, and an SO3 content ≤3.0%.
[0029] The low-carbon gel material comprises 80-85 wt% slag powder and steel slag powder, 8-12 wt% gypsum, 6.5-10.5 wt% alkaline activating material, and 0.5-0.8 wt% additives.
[0030] This application also provides a method for preparing the above-mentioned copper tailings slag-based road material, including the following steps:
[0031] S1, Preparation of low-carbon gel materials
[0032] Mix slag powder and steel slag powder in a ratio of 8:2, then add gypsum powder, alkaline activating material and additives, and mix evenly.
[0033] S2, Copper Tailings Preparation
[0034] The copper tailings slag is graded and dewatered through a sandblasting screen and a ceramic filter to control the copper tailings slag residue on a 200-mesh screen to be ≥40% and the moisture content to be ≤14%.
[0035] S3, Preparation of Road Materials from Copper Tailings Slag
[0036] The low-carbon gel material prepared in S1 was incorporated into the copper tailings slag prepared in S2 in a certain proportion, and the dosage of the gel material was detected by EDTA titration experiment. The dosage was controlled at 3-8 ± 0.2 wt%, and the overall moisture content was 8-12 wt%.
[0037] S4. The copper tailings slag road material prepared in S3 is paved, compacted, and cured. The paving thickness is controlled to ≤300mm; the compressibility coefficient is controlled to 1.6~1.8; two passes with a vibratory roller and two passes with a single / double drum roller are performed, with a compaction degree controlled to ≥93%; curing is carried out by watering or natural rainwater; 3-day core sampling is performed.
[0038] Copper tailings slag is a solid waste discharged by copper mining enterprises after mineral processing. Since the fineness and composition of copper tailings slag are similar to those of fly ash, referring to the core index requirements of fly ash for roadbed use in JTG / T F20-2015, the total content of CaO, SiO2, Al2O3, and MgO compounds in copper tailings is ≥70%, the loss on ignition is ≤20%, and the SO3 content is ≤3.0%. The main raw materials of solid waste-based cementitious materials are slag powder, steel slag powder, gypsum, and a small amount of alkaline activating materials and additives, which are crushed, ground, and mixed. The flexural strength of the mortar is ≥6MPa at 28d and the compressive strength is ≥32.5MPa at 28d.
[0039] Hydration mechanism of copper tailings slag and low-carbon cementitious materials: CaO in alkali-activated materials and CaO in slag powder or steel slag powder react with water: CaO + H2O → Ca(OH)2; SiO2 and Al2O3 provided by copper tailings slag, as well as active SiO2 and Al2O3 provided by slag powder, steel slag powder and alkali-activated materials, react under alkaline conditions: SiO2 + m1Ca(OH)2 + aq → m1CaO·SiO2·aq; Al2O3 + m2Ca(OH)2 + aq → m2Al2O3·SiO2·aq; Sulfate substances play a secondary activating role: Al2O3 + 3Ca(OH)2 + 3(CaSO4·2H2O) + aq → 3CaO·Al2O3·3CaSO4·32aq, 3CaO·Al2O3·3CaSO4. This compound is the main substance for forming strength.
[0040] This paper presents a novel copper tailings-based road material and its application method, developed by replacing traditional sand and gravel with copper tailings slag and cement with solid waste-based low-carbon cementitious materials, while considering construction costs and ensuring sustainable regional economic development. The applicant designed the aforementioned copper tailings-based road material. By designing the ratio of copper tailings slag to low-carbon cementitious materials and selecting optimal copper tailings slag and compatible low-carbon cementitious materials, a novel copper tailings-based road material suitable for road engineering was obtained. This material not only consumes copper tailings slag, reducing the cost of copper tailings treatment (30 yuan / ton), but also saves on the cost of stabilized crushed stone (98 yuan / ton). Furthermore, the material's core feature is that its 3-day unconfined compressive strength is comparable to the 7-day strength of traditional cement-stabilized crushed stone, allowing subsequent construction processes to be completed 4 days earlier than with cement-stabilized crushed stone, significantly shortening the construction period.
[0041] Unless otherwise specified, all materials used in the embodiments of this application are commercially available products.
[0042] Copper tailings slag: It needs to be treated by grading and dewatering (sandblasting screen and ceramic filter) with a residue of ≥40% on a 200-mesh sieve and a moisture content of ≤14%. It was purchased from Tongguan Lujiang Mining Company.
[0043] Steel slag powder: purchased from Baowu Group Environmental Resources Technology Co., Ltd.
[0044] Gypsum: Purchased from Anhui Hengtai New Materials Co., Ltd.
[0045] The alkaline activating material, i.e. the alkaline activator, is a mixture of sodium metasilicate, sodium silicate, and carbide slag, with the carbide slag being purchased from Anhui Huasheng Co., Ltd. of Huaibei Mining Group.
[0046] The admixture used in this application is, by way of, potassium aluminum sulfate and sodium thiosulfate; potassium aluminum sulfate is used by way of, by way of, an admixture used in this application. Specific Implementation
[0048] Preparation Examples 1-5 were used to prepare low-carbon gel materials.
[0049] Slag powder and steel slag powder were mixed at a ratio of 4:1, and then gypsum, alkaline activator, and additives were added and mixed evenly to obtain a low-carbon gel material. The mix proportions were optimized based on the baseline proportions from laboratory studies. The proportions of gypsum, alkaline activator, and additives added in each preparation example are shown in Table 1.
[0050] Table 1
[0051] Slag powder / wt% Steel slag powder / wt% Gypsum / wt% Excitation material / wt% Additives / wt% Preparation Example 1 68 17 8 6.5 0.5 Preparation Example 2 64 16 9 10.5 0.5 Preparation Example 3 65.6 16.4 10 7.5 0.5 Preparation Example 4 65.6 16.4 11 6.2 0.8 Preparation Example 5 64 16 12 7.5 0.5
[0052] Preparation Examples 6-10 were used to prepare copper tailings slag, controlling the moisture content of the copper tailings slag under different conditions. The moisture content of the copper tailings slag in each preparation example was as follows:
[0053] The copper tailings slag prepared in Example 6 had a moisture content of 6%.
[0054] The copper tailings slag prepared in Preparation Example 7 had a moisture content of 8%.
[0055] The copper tailings slag prepared in Example 8 has a moisture content of 10%.
[0056] The copper tailings slag prepared in Preparation Example 9 had a moisture content of 12%.
[0057] The copper tailings slag prepared in Preparation Example 10 had a moisture content of 14%.
[0058] The preparation of copper tailings slag-based road materials using the low-carbon gel materials prepared in Examples 1-5 and the copper tailings slag prepared in Examples 6-10 is shown in Table 2.
[0059] Table 2
[0060]
[0061]
[0062] The copper tailings slag-based road materials prepared in Examples 1-10 and the cement-stabilized crushed stone in the prior art were constructed according to the process described in Table 3. The unconfined compressive strength at 3 days was 1.0 MPa to 5.0 MPa, the unconfined compressive strength at 7 days was 1.5 MPa to 8 MPa, and the data at 28 days and 60 days showed a continuous increase.
[0063] Table 3
[0064]
[0065] As shown in Table 3, the copper tailings slag-based road materials prepared in Examples 1-10 of this application can be used for the next construction process after three days, which is four days earlier than the cement-stabilized crushed stone in the prior art. Therefore, it can be seen that using the copper tailings slag-based road materials prepared in this application can significantly reduce construction time and shorten the construction period compared to using the cement-stabilized crushed stone in the prior art.
[0066] The applicant analyzed the average value of the unconfined compressive strength of the copper tailings slag-based road materials in Examples 1 to 10 after construction, which was 3 / 7 days after construction. The average value is shown in Table 4.
[0067] Table 4
[0068] Copper tailings slag-based road materials 3-day unconfined compressive strength / MPa 7-day unconfined compressive strength / MPa Example 1 2.8 4.8 Example 2 4.2 7.5 Example 3 4.5 7.8 Example 4 4.1 7.3 Example 5 2.7 5.1 Example 6 2.9 4.9 Example 7 2.8 4.7 Example 8 4.6 7.8 Example 9 4.3 7.6 Example 10 4.4 7.5
[0069] As can be seen from Table 4 and Examples 1-5, the copper tailings-based road materials prepared using the low-carbon gel materials in Preparation Examples 2-4 and the copper tailings slag in Preparation Examples 7-9 have higher 3 / 7-day unconfined compressive strength.
[0070] Further examples 6-10 show that the variation in the 3 / 7-day unconfined compressive strength of copper tailings-based road materials is mainly due to the different types of copper tailings slag. The 3 / 7-day unconfined compressive strength of copper tailings-based road materials prepared using the copper tailings slag prepared in Examples 7-9 is higher. Therefore, it can be deduced that controlling the overall moisture content of copper tailings road materials to 8-12 wt% can result in better strength and construction performance of the prepared copper tailings-based road materials.
[0071] Based on the above, the applicant also tested the average freeze-thaw resistance and average strength loss rate of the copper tailings slag-based road materials prepared in Examples 1-10 after construction. The average freeze-thaw resistance and average strength loss rate of the copper tailings slag-based road materials prepared in Examples 11-20 of this application were ≤1.0% and ≤5.0% after construction.
[0072] Based on the above, the applicant also tested the road deflection value after construction of the copper tailings slag-based road material prepared in the embodiment, and the deflection value was ≤50 (0.01mm).
[0073] Based on the above, the applicant also tested the core samples (core drilling method) of the copper tailings slag-based road material prepared in the examples after construction. The unconfined compressive strength after construction was increased by 20% compared with the indoor unconfined compressive strength at all ages.
[0074] Based on the above, the applicant also conducted 28d / 60d / 90d / unconfined compressive strength tests on the copper tailings slag-based road material prepared in the examples, and the strength continued to increase.
[0075] Based on the above, the applicant also conducted groundwater environmental monitoring on the road sections using the copper tailings slag-based road material prepared in the embodiments. After implementation, the test data were collected for six months and one year, and compared with the original groundwater samples, there was no impact on the environment.
[0076] The above are all preferred embodiments of this application, and are not intended to limit the scope of protection of this application. Therefore, all equivalent changes made in accordance with the structure, shape and principle of this application should be covered within the scope of protection of this application.
Claims
1. A copper tailings slag-based road material, characterized in that, Includes 92-97 wt% copper tailings and 3-8 wt% low-carbon gel material; The copper tailings slag contains a total content of CaO, SiO2, Al2O3, and MgO compounds ≥70%, a moisture content of 8~12wt%, a loss on ignition ≤20%, and an SO3 content ≤3.0%. The low-carbon gel material comprises 80-85 wt% slag powder and steel slag powder, 8-12 wt% gypsum powder, 6.5-10.5 wt% alkaline activating material, and 0.5-0.8 wt% additives; The copper tailings residue on a 200-mesh sieve is ≥40%; The alkaline activating material is a mixture of sodium metasilicate, sodium silicate, and carbide slag in a ratio of 1:1:
8. The additive is one of potassium aluminum sulfate and sodium thiosulfate; The moisture content of the copper tailings slag road material is 8-12 wt%.
2. A method for preparing the copper tailings slag-based road material according to claim 1, characterized in that, Includes the following steps: S1, Preparation of low-carbon gel materials Mix slag powder and steel slag powder in a ratio of 8:2, then add gypsum powder, alkaline activating material and additives, and mix evenly. S2, Copper Tailings Preparation Copper tailings slag is graded and dewatered using a sandblasting screen and a ceramic filter to control the copper tailings slag residue on a 200-mesh sieve to be ≥40% and the moisture content to be 8~12wt%. S3, Preparation of Road Materials from Copper Tailings Slag The low-carbon gel material prepared in S1 was incorporated into the copper tailings slag prepared in S2 in a certain proportion, and the dosage of the gel material was detected by EDTA titration. The dosage was controlled at 3~8±0.2wt%, and the overall moisture content was 8~12wt%. S4. The copper tailings slag road material prepared in S3 is paved, compacted, and cured, with the paving thickness controlled ≤300mm; the shopu coefficient controlled 1.6~1.8; two passes with a vibratory roller and two passes with a single / double steel drum roller, with the compaction degree controlled ≥93%; curing by watering or natural rainwater; and 3-day core sampling.
3. The application of the copper tailings slag-based road material as described in claim 1 in the field of road engineering.
Citation Information
Patent Citations
Roadbed filling material and preparation method thereof
CN114436570A
Industrial solid waste-based green high-performance road cementing material and application thereof
CN115745432A