High-stability gel emulsion explosive and preparation method thereof

By adding modified nano-silica and antioxidants to gel-like emulsion explosives, the problems of decreased stability and oxidation reaction of gel-like emulsion explosives in humid environments are solved, achieving higher moisture resistance and oxidation resistance, and improving safety and stability.

CN118598722BActive Publication Date: 2026-11-20HENAN SONGGUANG CIVIL EXPLOSIVE EQUIP CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410783250.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2026-11-20
Estimated Expiration
2044-06-18

AI Technical Summary

Technical Problem

Gel-like emulsion explosives are prone to absorbing water in humid environments, which leads to decreased stability. Furthermore, the oxidizer and fuel are easily reacted with oxygen, posing safety hazards.

Method used

Highly stable colloidal emulsion explosives were prepared by adding modified nano-silica as a moisture-proofing agent and antioxidant. The modified nano-silica was oriented at the oil-water interface to form a stable water-in-oil structure, preventing water penetration and inhibiting oxidation reaction through the antioxidant.

Benefits of technology

It improves the moisture resistance and oxidation resistance of gelatinous emulsion explosives, extends their storage life, reduces the risk of accidental explosion and combustion, and ensures safety and stability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The application discloses a kind of high stability gel emulsion explosive and preparation method thereof, belong to the technical field of explosive, the gel emulsion explosive is by the following raw materials according to weight parts: ammonium nitrate 72~77 parts, sodium nitrate 6~8 parts, potassium nitrate 3~8 parts, water 10~15 parts, composite oil phase 6~6.5 parts, emulsifier 3~4 parts, sensitizer 1.6~1.8 parts, moisture-proof agent 0.5~0.8, antioxidant 0.2~0.4 parts.The gel emulsion explosive prepared by the application has good explosion performance, good moisture resistance, good oxidation resistance, high chemical stability and long storage time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of explosives technology, specifically relating to a highly stable gelatinous emulsion explosive and its preparation method. Background Technology

[0002] Gel-like emulsion explosives are a common type of industrial explosive, widely used in mining, infrastructure construction, and other fields. They are composed of oxidizers, fuels, emulsifiers, sensitizers, stabilizers, and water, manufactured through a specific process. The oxidizer and fuel are the main sources of explosive energy; the emulsifier stabilizes the emulsion structure, reducing the risk of accidental explosions; the sensitizer enables rapid detonation upon stimulation, ensuring effective blasting; furthermore, gel-like emulsion explosives possess strong resistance to deflagration, maintaining stable performance in complex blasting environments and exhibiting high safety.

[0003] However, in practical applications, gelatinous emulsion explosives also face some challenges, especially their strong water absorption and sensitivity to oxidation. First, gelatinous emulsion explosives exhibit significant water absorption due to their unique physical and chemical properties. In humid environments, the explosives easily absorb moisture from the air. Once this moisture enters the explosive system, it reacts with certain components, leading to decreased stability and potentially reduced explosive performance. More seriously, the presence of moisture may increase the risk of accidental explosion or combustion during use, threatening personnel safety and equipment stability. Second, oxidizers and fuels in gelatinous emulsion explosives are prone to slow oxidation reactions with oxygen in the air during prolonged storage or under adverse conditions. This oxidation reaction gradually alters the chemical properties of the explosive, causing a gradual decline in its performance. If the oxidation reaction reaches a certain level, it may even trigger spontaneous combustion or explosion, posing serious safety hazards.

[0004] Therefore, developing a highly stable gel-like emulsion to improve its moisture resistance and antioxidant properties has become one of the problems that urgently need to be solved by those skilled in the art. Summary of the Invention

[0005] In view of the shortcomings of the prior art, the present invention discloses a highly stable gel-like emulsion explosive and its preparation method. By adding appropriate moisture-proofing agents and antioxidants, the safety and effectiveness of the gel-like emulsion explosive in actual use are guaranteed.

[0006] This invention discloses a highly stable gelatinous emulsion explosive, which is composed of the following raw materials by weight: 72-77 parts ammonium nitrate, 6-8 parts sodium nitrate, 3-8 parts potassium nitrate, 10-15 parts water, 6-6.5 parts composite oil phase, 3-4 parts emulsifier, 1.6-1.8 parts sensitizer, 0.5-0.8 parts moisture-proof agent, and 0.2-0.4 parts antioxidant.

[0007] Preferably, the composite oil phase is composed of liquid paraffin, petrolatum, silicone oil and chlorinated paraffin, and the mass ratio of liquid paraffin, petrolatum, silicone oil and chlorinated paraffin is 6:5:2:5.

[0008] Preferably, the preparation method of the composite oil phase includes the following steps: liquid paraffin, petrolatum, silicone oil and chlorinated paraffin are placed in an oil phase tank according to the mass ratio, stirred and heated to 90℃~95℃, and kept at the temperature for 20~30min to obtain the composite oil phase.

[0009] Preferably, the emulsifier is composed of polyisobutylene succinimide, polyglycerol fatty acid ester, soybean lecithin, and sorbitol monooleate; the mass ratio of polyisobutylene succinimide, polyglycerol fatty acid ester, soybean lecithin, and sorbitol monooleate is 1:2:3:9.

[0010] Preferably, the sensitizer is one of dinitrosopeptimethylenetetramine and sodium nitrite; the antioxidant is one of butylated hydroxyanisole and dibutylated hydroxytoluene; and the moisture-proofing agent is modified nano-silica.

[0011] Preferably, the preparation method of the modified nano-silica includes the following steps: After cleaning and drying the nano-silica, it is slowly added to a beaker containing anhydrous ethanol solution of silane coupling agent KH-550. The beaker is placed on a constant temperature magnetic stirrer and the modification reaction is carried out at 60-80°C. After the reaction is carried out for 2-3 hours, it is washed and dried to obtain the modified nano-silica.

[0012] Preferably, the mass ratio of the silane coupling agent KH-550 to anhydrous ethanol is (1-5):100; and the mass ratio of the silane coupling agent KH-550 to nano-silica is (0.02-0.04):1.

[0013] This invention also provides a method for preparing the above-mentioned highly stable gelatinous emulsion explosive, comprising the following steps:

[0014] S1. According to the weight ratio, ammonium nitrate, sodium nitrate, potassium nitrate and water are placed in an aqueous phase dissolution tank, stirred and heated to 90-100℃, and kept at the temperature for 40-45 minutes to obtain an aqueous phase;

[0015] S2. According to the weight ratio, the composite oil phase, emulsifier, antioxidant and the aqueous phase obtained in step S1 are placed in an emulsification device for emulsification to obtain a latex matrix;

[0016] S3. The sensitizer, the latex matrix obtained in step S2 and the moisture-proof agent are added to the sensitization device for sensitization, that is: to obtain a highly stable gel-like emulsion explosive;

[0017] S4. The gelatinous emulsion explosive obtained in step S3 is loaded into explosive rolls of different specifications using a loading machine to obtain the finished product.

[0018] Preferably, the emulsification temperature in step S2 is 90–100°C; the sensitization temperature in step S3 is 47–53°C; and the drug loading temperature in step S4 is 45–50°C.

[0019] Preferably, the technical indicators of the high-stability gel-like emulsion explosive product obtained in step S4 are as follows: working capacity (mL): ≥220; detonation velocity (m / s): 3200≤V≤4500; sympathetic detonation distance (cm): ≥6; toxic gas content (L / Kg): ≤70.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] (1) This invention, by adding modified nano-silica, not only enables the prepared gel-like emulsion explosive to have good moisture resistance, but also improves the overall stability of the emulsion explosive. Gel-like emulsion explosives are usually water-in-oil structures. In the preparation process of gel-like emulsion explosives, the emulsifier, as a surfactant, is oriented at the oil-water interface, with its hydrophobic end pointing towards the oil phase and its hydrophilic end extending into the water phase, forming a stable water-in-oil (W / O) emulsion system, thereby ensuring the stability of the emulsion explosive. This invention modifies nano-silica using the silane coupling agent KH-550. The modified nano-silica surface is effectively coated with KH-550, and two different groups (one hydrophobic siloxane and the other hydrophilic amino) are grafted onto its surface, giving the modified nano-silica both oleophilic and hydrophilic properties. In the preparation of gel-like emulsion explosives, its hydrophobic portion points towards the oil phase, while its hydrophilic portion extends into the aqueous phase. It can be oriented at the oil-water interface like an emulsifier, maintaining the stability of the emulsion system. Furthermore, through the characteristics of its hydrophilic end, it can form a barrier to prevent or slow down the penetration of external moisture into the emulsion explosive, thus preventing the destruction of the originally stable water-in-oil (W / O) structure. It has excellent hydrophobicity and strong interfacial activity, effectively improving the moisture-proof performance of gel-like emulsion explosives.

[0022] (2) The gelatinous emulsion explosive disclosed in this invention contains antioxidants butylated hydroxyanisole (BHA) or butylated hydroxytoluene (BHT). When explosives or other oily substances are exposed to oxygen, they may undergo auto-oxidation, generating free radicals. These free radicals attack molecular chains, triggering a chain reaction of oxidation. The hydroxyl (-OH) groups of BHA or BHT can contribute their hydrogen atoms to the free radicals, combining with them to stop the free radical chain reaction, thereby protecting the explosives or other substances from oxidative damage. Furthermore, oxidants (such as nitrates) and fuels in explosives are prone to slow oxidation reactions with oxygen in the air due to long-term storage, forming unstable peroxides. BHA or BHT can further react with these peroxides, preventing them from decomposing and generating more free radicals, thereby reducing oxidative damage. By adding antioxidants during the preparation of gelatinous emulsion explosives, this invention effectively inhibits or slows down the oxidation process of explosive components, improves the chemical stability of gelatinous emulsion explosives, and extends their shelf life. Detailed Implementation

[0023] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0024] This invention discloses a highly stable gelatinous emulsion explosive, which is composed of the following raw materials in parts by weight: 72-77 parts ammonium nitrate, 6-8 parts sodium nitrate, 3-8 parts potassium nitrate, 10-15 parts water, 6-6.5 parts composite oil phase, 3-4 parts emulsifier, 1.6-1.8 parts sensitizer, 0.5-0.8 parts moisture-proof agent, and 0.2-0.4 parts antioxidant.

[0025] The composite oil phase consists of liquid paraffin, petrolatum, silicone oil, and chlorinated paraffin in a mass ratio of 6:5:2:5; the emulsifier consists of polyisobutylene succinimide, polyglycerol fatty acid ester, soybean lecithin, and dehydrated sorbitan monooleate in a mass ratio of 1:2:3:9; the sensitizer is one of dinitrosopeptimide and sodium nitrite; the antioxidant is one of butylated hydroxyanisole and dibutylated hydroxytoluene; and the moisture-proofing agent is modified nano-silica.

[0026] The preparation method of the above-mentioned composite oil phase in this embodiment is as follows: liquid paraffin, petrolatum, silicone oil and chlorinated paraffin are placed in an oil phase tank according to the mass ratio, stirred and heated to 90℃~95℃, and kept at the temperature for 20~30min to obtain the composite oil phase.

[0027] The preparation method of the modified nano-silica in this embodiment is as follows: After cleaning and drying the nano-silica, it is slowly added to a beaker containing anhydrous ethanol solution of silane coupling agent K-H550. The beaker is placed on a constant temperature magnetic stirrer and the modification reaction is carried out at 60-80℃. After the reaction is carried out for 2-3 hours, it is washed and dried to obtain the modified nano-silica.

[0028] The mass ratio of silane coupling agent KH-550 to anhydrous ethanol is (1-5):100, and the mass ratio of silane coupling agent KH-550 to nano-silica is (0.02-0.04):1.

[0029] The preparation method of the above-mentioned highly stable gelatinous emulsion explosive in this embodiment includes the following steps:

[0030] S1. According to the weight ratio, ammonium nitrate, sodium nitrate, potassium nitrate and water are placed in an aqueous phase dissolution tank, stirred and heated to 90-100℃, and kept at the temperature for 40-45 minutes to obtain an aqueous phase.

[0031] S2. According to the weight ratio, the composite oil phase, emulsifier, antioxidant and the aqueous phase obtained in step S1 are placed in an emulsification device and emulsified at 90-100°C to obtain a latex matrix.

[0032] S3. Add the sensitizer, latex matrix and moisture-proofing agent to the sensitization device and sensitize at 47-53°C to obtain a highly stable gel-like emulsion explosive.

[0033] S4. The gelatinous emulsion explosive obtained in step S3 is loaded into explosive rolls of different specifications at 45-50°C using a loading machine to obtain the finished product.

[0034] The technical specifications of the high-stability gel-like emulsion explosive product obtained above are as follows: work capacity (mL): ≥220; detonation velocity (m / s): 3200≤V≤4500; sympathetic detonation distance (cm): ≥6; toxic gas content (L / Kg): ≤70.

[0035] The technical solution of the present invention will be further described below with reference to specific embodiments:

[0036] Example 1

[0037] The preparation method of the composite oil phase in this embodiment is as follows: liquid paraffin, petrolatum, silicone oil and chlorinated paraffin are placed in an oil phase tank at a mass ratio of 6:5:2:5, stirred and heated to 93°C, and kept at the temperature for 25 minutes to obtain the composite oil phase.

[0038] The preparation method of modified nano-silica in this embodiment is as follows: After cleaning and drying pretreatment, nano-silica (nano-silica: KH-550 = 1: 0.03) is slowly added to a beaker containing anhydrous ethanol solution of silane coupling agent KH-550 (KH-550: anhydrous ethanol = 1: 50). The beaker is placed on a constant temperature magnetic stirrer and the modification reaction is carried out at 70°C. After the reaction is carried out for 2.5 hours, it is washed and dried to obtain modified nano-silica.

[0039] The preparation method of the highly stable gelatinous emulsion explosive in this embodiment includes the following specific steps:

[0040] S1. Place 76 parts of ammonium nitrate, 7 parts of sodium nitrate, 5 parts of potassium nitrate and 10 parts of water into an aqueous phase dissolution tank, stir and heat to 95°C, keep warm for 42 minutes to obtain an aqueous phase.

[0041] S2. Place 6.2 parts of the composite oil phase, 3.5 parts of the emulsifier, 0.3 parts of butylated hydroxyanisole, and the aqueous phase obtained in step S1 into an emulsification device and emulsify at 96°C to obtain a latex matrix.

[0042] The emulsifier is composed of polyisobutylene succinimide, polyglycerol fatty acid ester, soybean lecithin, and dehydrated sorbitan monooleate in a mass ratio of 1:2:3:9.

[0043] S3. Add 1.75 parts of dinitrosopeptimide, the latex matrix obtained in step S2 and 0.6 parts of modified nano-silica to the sensitization device and sensitize at 49°C to obtain a highly stable gel-like emulsion explosive.

[0044] S4. The gelatinous emulsion explosive obtained in step S3 is loaded into explosive rolls of different specifications at 48°C using a loading machine to obtain the finished product.

[0045] The gelatinous emulsion explosive prepared in this embodiment can be stored for 6 to 8 months, and its performance remains stable during storage.

[0046] The technical specifications of the high-stability gel-like emulsion explosive product prepared in this embodiment are as follows: work capacity (mL): 255; detonation velocity (m / s): 4750; sympathetic detonation distance (cm): 6; toxic gas content (L / Kg): 20.

[0047] Example 2

[0048] The preparation method of the composite oil phase in this embodiment is as follows: liquid paraffin, petrolatum, silicone oil and chlorinated paraffin are placed in an oil phase tank at a mass ratio of 6:5:2:5, stirred and heated to 90°C, and kept at that temperature for 30 minutes to obtain the composite oil phase.

[0049] The preparation method of modified nano-silica in this embodiment is as follows: After cleaning and drying pretreatment, nano-silica (nano-silica: KH-550 = 1: 0.02) is slowly added to a beaker containing anhydrous ethanol solution of silane coupling agent KH-550 (KH-550: anhydrous ethanol = 1: 100). The beaker is placed on a constant temperature magnetic stirrer and the modification reaction is carried out at 60°C. After the reaction is carried out for 3 hours, it is washed and dried to obtain modified nano-silica.

[0050] The preparation method of the highly stable gelatinous emulsion explosive in this embodiment includes the following specific steps:

[0051] S1. Place 74 parts of ammonium nitrate, 6.5 parts of sodium nitrate, 6 parts of potassium nitrate and 12 parts of water into an aqueous phase dissolution tank, stir and heat to 90°C, keep warm for 45 minutes to obtain an aqueous phase.

[0052] S2. Place 6.3 parts of the composite oil phase, 3 parts of the emulsifier, 0.2 parts of butylated hydroxytoluene and the aqueous phase obtained in step S1 into an emulsification device and emulsify at 90°C to obtain a latex matrix.

[0053] The emulsifier is composed of polyisobutylene succinimide, polyglycerol fatty acid ester, soybean lecithin, and dehydrated sorbitan monooleate in a mass ratio of 1:2:3:9.

[0054] S3. Add 1.6 parts of sodium nitrite, the latex matrix obtained in step S2 and 0.5 parts of modified nano-silica to the sensitization device and sensitize at 47°C to obtain a highly stable gel-like emulsion explosive.

[0055] S4. The gelatinous emulsion explosive obtained in step S3 is loaded into explosive rolls of different specifications at 45°C using a loading machine to obtain the finished product.

[0056] The gelatinous emulsion explosive prepared in this embodiment can be stored for 6 to 8 months, and its performance remains stable during storage.

[0057] The technical specifications of the high-stability gel-like emulsion explosive product prepared in this embodiment are as follows: work capacity (mL): 270; detonation velocity (m / s): 4800; sympathetic detonation distance (cm): 6; toxic gas content (L / Kg): 25.

[0058] Example 3

[0059] The preparation method of the composite oil phase in this embodiment is as follows: liquid paraffin, petrolatum, silicone oil and chlorinated paraffin are placed in an oil phase tank at a mass ratio of 6:5:2:5, stirred and heated to 95°C, and kept at that temperature for 20 minutes to obtain the composite oil phase.

[0060] The preparation method of modified nano-silica in this embodiment is as follows: After cleaning and drying pretreatment, nano-silica (nano-silica: KH-550 = 1:0.04) is slowly added to a beaker containing anhydrous ethanol solution of silane coupling agent KH-550 (KH-550: anhydrous ethanol = 1:20). The beaker is placed on a constant temperature magnetic stirrer and the modification reaction is carried out at 70°C. After the reaction is carried out for 2.5 hours, it is washed and dried to obtain modified nano-silica.

[0061] The preparation method of the highly stable gelatinous emulsion explosive in this embodiment includes the following specific steps:

[0062] S1. Place 76 parts of ammonium nitrate, 7.5 parts of sodium nitrate, 7 parts of potassium nitrate and 15 parts of water into an aqueous phase dissolution tank, stir and heat to 100°C, keep warm for 40 minutes to obtain an aqueous phase.

[0063] S2. Place 6.1 parts of the composite oil phase, 4 parts of the emulsifier, 0.4 parts of butylated hydroxyanisole and the aqueous phase obtained in step S1 into an emulsification device and emulsify at 100°C to obtain a latex matrix.

[0064] The emulsifier is composed of polyisobutylene succinimide, polyglycerol fatty acid ester, soybean lecithin, and dehydrated sorbitan monooleate in a mass ratio of 1:2:3:9.

[0065] S3. Add 1.8 parts of dinitrosopeptimide, the latex matrix obtained in step S2 and 0.8 parts of modified nano-silica to the sensitization device and sensitize at 53°C to obtain a highly stable gel-like emulsion explosive.

[0066] S4. The gelatinous emulsion explosive obtained in step S3 is loaded into explosive rolls of different specifications at 50°C using a loading machine to obtain the finished product.

[0067] The gelatinous emulsion explosive prepared in this embodiment can be stored for 6 to 8 months, and its performance remains stable during storage.

[0068] The technical specifications of the high-stability gel-like emulsion explosive product prepared in this embodiment are as follows: work capacity (mL): 280; detonation velocity (m / s): 4900; sympathetic detonation distance (cm): 6; toxic gas content (L / Kg): 23.

[0069] The above provides a detailed description of a highly stable gelatinous emulsion explosive and its preparation method disclosed in this invention. Specific examples have been used to illustrate the principles and implementation methods of this invention. The descriptions of the above embodiments are merely for the purpose of helping to understand the method and core ideas of this invention. It should be noted that those skilled in the art can make various improvements and modifications to this invention without departing from its principles, and these improvements and modifications also fall within the protection scope of the claims of this invention.

Claims

1. A highly stable gelatinous emulsion explosive, characterized in that, The gelatinous emulsion explosive is composed of the following raw materials by weight: 72-77 parts ammonium nitrate, 6-8 parts sodium nitrate, 3-8 parts potassium nitrate, 10-15 parts water, 6-6.5 parts composite oil phase, 3-4 parts emulsifier, 1.6-1.8 parts sensitizer, 0.5-0.8 parts moisture-proof agent, and 0.2-0.4 parts antioxidant; the sensitizer is one of dinitrosopeptimethylenetetramine and sodium nitrite; the antioxidant is one of butylated hydroxyanisole and dibutylated hydroxytoluene; and the moisture-proof agent is modified nano-silica. The preparation method of the modified nano-silica is as follows: After cleaning and drying pretreatment, the nano-silica is slowly added to a beaker containing anhydrous ethanol solution of silane coupling agent K-H550. The beaker is placed on a constant temperature magnetic stirrer and the modification reaction is carried out at 60~80℃. After the reaction is carried out for 2~3 hours, it is washed and dried to obtain the modified nano-silica.

2. The highly stable gelatinous emulsion explosive according to claim 1, characterized in that, The composite oil phase is composed of liquid paraffin, petrolatum, silicone oil and chlorinated paraffin, and the mass ratio of liquid paraffin, petrolatum, silicone oil and chlorinated paraffin is 6:5:2:

5.

3. The highly stable gelatinous emulsion explosive according to claim 2, characterized in that, The preparation method of the composite oil phase is as follows: liquid paraffin, petrolatum, silicone oil and chlorinated paraffin are placed in an oil phase tank according to the mass ratio, stirred and heated to 90℃~95℃, and kept at the temperature for 20~30min to obtain the composite oil phase.

4. The highly stable gelatinous emulsion explosive according to claim 1, characterized in that, The emulsifier is composed of polyisobutylene succinimide, polyglycerol fatty acid ester, soybean lecithin, and sorbitol monooleate; the mass ratio of polyisobutylene succinimide, polyglycerol fatty acid ester, soybean lecithin, and sorbitol monooleate is 1:2:3:

9.

5. The highly stable gelatinous emulsion explosive according to claim 1, characterized in that, The mass ratio of the silane coupling agent KH-550 to anhydrous ethanol is (1~5):100; the mass ratio of the silane coupling agent KH-550 to nano-silica is (0.02~0.04):

1.

6. The method for preparing the highly stable colloidal emulsion explosive according to any one of claims 1-5, characterized in that, Includes the following steps: S1. According to the weight ratio, ammonium nitrate, sodium nitrate, potassium nitrate and water are placed in an aqueous phase dissolution tank, stirred and heated to 90~100℃, and kept at the temperature for 40~45min to obtain an aqueous phase; S2. According to the weight ratio, the composite oil phase, emulsifier, antioxidant and the aqueous phase obtained in step S1 are placed in an emulsification device for emulsification to obtain a latex matrix; S3. The sensitizer, the latex matrix obtained in step S2 and the moisture-proof agent are added to the sensitization device for sensitization, that is: to obtain a highly stable gel-like emulsion explosive; S4. The gelatinous emulsion explosive obtained in step S3 is loaded into explosive rolls of different specifications using a loading machine to obtain the finished product.

7. The method for preparing a highly stable colloidal emulsion explosive according to claim 6, characterized in that, The emulsification temperature in step S2 is 90~100℃; the sensitization temperature in step S3 is 47~53℃; and the drug loading temperature in step S4 is 45~50℃.

8. The method for preparing a highly stable colloidal emulsion explosive according to claim 7, characterized in that, The technical specifications of the high-stability gel-like emulsion explosive product obtained in step S4 are as follows: work capacity (mL): ≥220; detonation velocity (m / s): 3200≤V≤4500; sympathetic detonation distance (cm): ≥6; toxic gas content (L / Kg): ≤70.

Citation Information

Patent Citations

  • Emulsified explosive dedicated complex lipid prepared by waste animal and plant greases and preparation method thereof

    CN103964981A

  • Modified nano-titanium dioxide with tenacity and good damp-proof effect, and preparation method of modified nano-titanium dioxide