A 9-phenyl-9h-carbazole group modified graphite phase carbon nitride yellow-green light material

The preparation of graphitic carbon nitride modified with 9-phenyl-9H-carbazole group by high-temperature solid-state reaction method solves the problem of synthesizing long-wavelength fluorescent materials in the prior art, and realizes the simple and low-cost preparation of yellow-green fluorescent materials and the redshift effect of emission peak.

CN118599530BActive Publication Date: 2026-11-24YUNNAN MINZU UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410782467.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2026-11-24
Estimated Expiration
2044-06-18

AI Technical Summary

Technical Problem

Existing technologies make it difficult to synthesize graphitic carbon nitride materials that emit long-wavelength fluorescence other than blue light easily and at low cost, especially yellow-green fluorescent materials, and the existing methods have harsh reaction conditions.

Method used

A high-temperature solid-phase reaction method was adopted, using melamine and 6-(4-(9H-carbazole-9-yl)phenyl)-1,3,5-triazine-2,4-diamine as raw materials. After grinding and mixing, the mixture was calcined at 450 °C under nitrogen protection to prepare graphitic carbon nitride modified with 9-phenyl-9H-carbazole group.

Benefits of technology

A yellow-green fluorescent material was successfully synthesized, with the emission peak significantly red-shifted to 470~700 nm and the luminescence intensity significantly enhanced, achieving a simple and low-cost preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

A type of 9-phenyl-9 H A method for preparing yellow-green luminescent materials of graphitic carbon nitride derivatives modified with α-carbazole groups. Melamine is used as the main raw material, 6-(4-(9) H 9-Carbazole-9-yl)phenyl)-1,3,5-triazine-2,4-diamine was used as a dopant and mixed uniformly at a certain molar ratio. The mixture was then polymerized at 450 °C for 2 hours under nitrogen protection to obtain 9-phenyl-9-yl)phenyl)-1,3,5-triazine-2,4-diamine. H A yellow-green fluorescent material derived from graphitic carbon nitride modified with a 9-carbazole group. The fluorescent material prepared in this invention emits in the 470-700 nm range, with a maximum emission wavelength of approximately 559 nm. Compared to unmodified graphitic carbon nitride, the maximum emission wavelength is red-shifted by about 108 nm, and the luminescence intensity is significantly improved. The 9-phenyl-9-carbazole group obtained in this invention... H Yellow-green light materials derived from graphitic carbon nitride modified with α-carbazole groups have advantages such as short process flow, fewer equipment required, low cost, and high temperature resistance, and have potential application value in fields such as phosphors, chemical sensing, and bioimaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of materials preparation, specifically relating to a graphitic carbon nitride derivative yellow-green light material modified with a 9-phenyl-9H-carbazole group and its preparation method. Background Technology

[0002] Graphitic carbon nitride (g-C3N4) is an excellent two-dimensional layered material that is easy to synthesize, highly stable, safe, and non-toxic, and has good application value in catalysis, energy storage, adsorption, separation, and luminescence. Graphitic carbon nitride is easy and inexpensive to synthesize, and can be directly polymerized from melamine, dicyandiamide, cyanamide, urea, thiourea, etc., indicating that it can be mass-produced.

[0003] Graphitic carbon nitride, as a luminescent material, possesses advantages such as high temperature resistance, abundant raw materials, low cost, high fluorescence intensity, and good biocompatibility, and has found good applications in fluorescent materials, bioimaging, sensing, and fingerprint recognition. Its photoluminescence spectrum is located in the blue light region, typically between 430 and 550 nm, with a maximum emission wavelength around 470 nm [Liu J, Wang H, Antonietti M. Graphitic carbon nitride 'reloaded': emerging applications beyond (photo)catalysis[J]. Chemical Society Reviews, 2016, 45, 2308–2326]. Graphitic carbon nitride can be directly used as a blue light material. Currently, research and applications of modified graphitic carbon nitride for use as green, red, and yellow fluorescent materials are limited, while these colored luminescent materials have significant application value in many fields; therefore, there is still considerable room for improvement. There are two main methods to control the emission wavelength of graphitic carbon nitride: First, introducing aromatic rings (such as benzene rings) into the conjugated structure of graphitic carbon nitride will cause the π-electron conjugated system of graphitic carbon nitride to become larger and the band narrower, resulting in a red shift in the fluorescence spectrum of graphitic carbon nitride [Cui Q, Xu J, Wang X, et al. Phenyl-modified carbon nitride quantum dots with distinct photoluminescence behavior[J]. Angewandte Chemie, 2016, 128(11):3736–3740;CN106833609A]. Second, non-metallic elements with low electronegativity and large radius, such as P and S, are incorporated into graphitic carbon nitride by doping, thereby changing the maximum emission peak of graphitic carbon nitride [Jiang W, Yang S, Li J, et al. Electron injection of phosphorus doped g-C3N4 quantum dots: controllable photoluminescence emission wavelength in the whole visible light range with high quantum yield[J]. Advanced Optical Materials, 2016, 4, 2095–2101].However, the methods for synthesizing graphitic carbon nitride derivatives mentioned in the above literature all require pretreatment followed by high-temperature calcination or reaction in a reactor to obtain the product, making the process and reaction conditions quite demanding. Therefore, developing a graphitic carbon nitride with a simple synthesis process, low cost, and the ability to emit long-wavelength fluorescence other than blue light has significant research value and application prospects. Summary of the Invention

[0004] The purpose of this invention is to provide a simple method for preparing graphite-phase carbon nitride-based yellow-green fluorescent materials.

[0005] The raw materials required for this invention are melamine and 6-(4-(9H-carbazole-9-yl)phenyl)-1,3,5-triazine-2,4-diamine, with melamine being the main raw material and 6-(4-(9H-carbazole-9-yl)phenyl)-1,3,5-triazine-2,4-diamine being the dopant.

[0006] To achieve the above objectives, the preparation method adopted in this invention is a high-temperature solid-phase reaction method, the specific steps of which are as follows: melamine and 6-(4-(9H-carbazole-9-yl)phenyl)-1,3,5-triazine-2,4-diamine are mixed evenly by grinding at a certain molar ratio (or corresponding mass ratio), the mixture is placed in a crucible, and calcined at 450 °C for 2 hours under nitrogen protection. After the reaction is completed, it is cooled to room temperature to obtain a yellow powder product. Attached Figure Description

[0007] Figure 1 A schematic diagram of the synthesis of graphitic carbon nitride modified with a 9-phenyl-9H-carbazole group.

[0008] Figure 2 The graphitic carbon nitride modified with the 9-phenyl-9H-carbazole group obtained in Example 1 13 The C solid-state nuclear magnetic resonance spectrum, with the inset showing representative structural units of the polymer.

[0009] Figure 3 The image shows a comparison of the infrared spectra of the graphitic carbon nitride modified with the 9-phenyl-9H-carbazole group obtained in Example 1 and the unmodified graphitic carbon nitride obtained in the comparative example.

[0010] Figure 4The photoluminescence emission spectra of graphitic carbon nitride modified with 9-phenyl-9H-carbazole groups synthesized by doping with different amounts of 6-(4-(9H-carbazole-9-yl)phenyl)-1,3,5-triazine-2,4-diamine (Examples 1, 2, and 3) are compared with those of unmodified graphitic carbon nitride powder (Comparative Example). The excitation wavelength of the product obtained in Example 1 is 415 nm, the excitation wavelength of the product obtained in Example 2 is 420 nm, the excitation wavelength of the product obtained in Example 3 is 411 nm, and the excitation wavelength of the Comparative Example is 350 nm. Detailed Implementation

[0011] Example 1 Melamine and 6-(4-(9H-carbazole-9-yl)phenyl)-1,3,5-triazine-2,4-diamine were mixed at a molar ratio of 30:1. 0.30 g of melamine and 0.028 g of 6-(4-(9H-carbazole-9-yl)phenyl)-1,3,5-triazine-2,4-diamine were weighed and ground in an agate mortar for 30 minutes. The mixture was then placed in a corundum crucible and reacted at 450 °C under nitrogen protection for 2 hours. The resulting yellow powder was a 9-phenyl-9H-carbazole group-modified graphitic carbon nitride yellow-green fluorescent material.

[0012] Example 2 Melamine and 6-(4-(9H-carbazole-9-yl)phenyl)-1,3,5-triazine-2,4-diamine were weighed at a molar ratio of 20:1. 0.30 g of melamine and 0.042 g of 6-(4-(9H-carbazole-9-yl)phenyl)-1,3,5-triazine-2,4-diamine were ground in a mortar for 30 minutes, then placed in a corundum crucible and reacted at 450 °C under nitrogen protection for 2 hours. The resulting yellow powder was a 9-phenyl-9H-carbazole group-modified graphitic carbon nitride yellow-green fluorescent material.

[0013] Example 3 Melamine and 6-(4-(9H-carbazole-9-yl)phenyl)-1,3,5-triazine-2,4-diamine were mixed at a molar ratio of 40:1. 0.30 g of melamine and 0.021 g of 6-(4-(9H-carbazole-9-yl)phenyl)-1,3,5-triazine-2,4-diamine were weighed and ground in a mortar for 30 minutes. The mixture was then placed in a corundum crucible and reacted at 450 °C under nitrogen protection for 2 hours. The resulting yellow powder was a 9-phenyl-9H-carbazole group-modified graphitic carbon nitride yellow-green fluorescent material.

[0014] Comparison Examples 1.5 g of melamine was weighed, ground, and transferred into a corundum crucible. The mixture was reacted at 450 °C under nitrogen protection for 2 hours, and the resulting yellow powder was unmodified graphitic carbon nitride.

[0015] Figure 1 A schematic diagram of the synthesis of graphitic carbon nitride yellow-green fluorescent material modified with 9-phenyl-9H-carbazole group.

[0016] Figure 2 The graphitic carbon nitride yellow-green fluorescent material (g-C3N4-Cz-Ph) modified with the 9-phenyl-9H-carbazole group obtained in Example 1 is shown. 30:1 )of 13 C solid-state nuclear magnetic resonance spectrum ( 13 (CSSNMR), the two strong peaks on the left side of the spectrum are g-C3N4-Cz-Ph 30:1 The signal peaks of the C atom on the heptaazine ring appear at approximately 164.6 ppm and 155.1 ppm, respectively, and belong to the carbon atoms identified as a and b in the illustration. The other peaks are NMR signal peaks of the carbon atom in the 9-phenyl-9H-carbazole group, corresponding to... Figure 2 The carbon atoms numbered c (140.3 ppm), d (130.2 ppm), e (124.1 ppm), f (120.3 ppm), and g (109.0 ppm) are representative structural units. Based on the combined spectral results, the 9-phenyl-9H-carbazole group has been successfully grafted onto the heptaazine ring of graphitic carbon nitride, followed by g-C3N4-Cz-Ph 30:1 The FT-IR spectrum also confirms this conclusion.

[0017] Figure 3 The image shows a comparison of the infrared spectra of the 9-phenyl-9H-carbazole group-modified yellow-green fluorescent material of graphitic carbon nitride obtained in Example 1 and the unmodified graphitic carbon nitride powder obtained in the comparative example. The spectra are at 803 cm⁻¹. -1 Both spectra show moderate absorption peaks, typical of the stretching vibrations of the heptaazine ring; 1750–1360 cm⁻¹ -1 There are two strong peaks between 3500 and 3300 cm⁻¹, which are absorption peaks generated by the C–N / C=N stretching vibration of the heptaazine ring. -1The stretching vibration peaks of NH are present in all three locations, originating from the completely reacted −NH2 and >NH at the edges or defect regions of the two-dimensional graphitic carbon nitride sheets. The fact that the infrared absorption peaks of the 9-phenyl-9H-carbazole group-modified graphitic carbon nitride and the unmodified graphitic carbon nitride are roughly the same indicates that the modified graphitic carbon nitride still uses the heptaazine ring as the main structure, accounting for the majority of the molecular structure. The infrared spectrum of the 9-phenyl-9H-carbazole group-modified graphitic carbon nitride shows a peak at 3060 cm⁻¹. -1 The infrared spectrum of graphitic carbon nitride shows obvious absorption peaks on both sides that are different from those of unmodified graphitic carbon nitride. The stretching vibration of CH on the benzene ring of the 9-phenyl-9H-carbazole group further indicates that the 9-phenyl-9H-carbazole group was successfully grafted onto the heptaazine ring of graphitic carbon nitride.

[0018] Figure 4 This is a comparison of the fluorescence spectra of the 9-phenyl-9H-carbazole-modified yellow-green fluorescent materials of graphitic carbon nitride prepared by doping different amounts of 6-(4-(9H-carbazole-9-yl)phenyl)-1,3,5-triazine-2,4-diamine in Examples 1, 2, and 3, and the unmodified graphitic carbon nitride powder obtained in the comparative examples. Figure 4 It can be seen that, compared with unmodified graphitic carbon nitride powder emitting blue light (mainly emitted at 375~550 nm, with maximum emission at 451 nm), the yellow-green fluorescent material prepared in this invention emits light mainly at 470~700 nm, with a significant redshift of the strongest emission peak. The maximum emission of the products obtained in Examples 1, 2, and 3 is located at 559 nm, 562 nm, and 555 nm, respectively, representing redshifts of 108 nm, 111 nm, and 104 nm. Meanwhile, the luminescence intensity of the products obtained in Examples 1, 2, and 3 after modification with the 9-phenyl-9H-carbazole group is significantly enhanced. Comparatively, the product obtained in Example 1 has the strongest luminescence intensity and is the best product.

Claims

1. A 9-phenyl-9 H- A carbazole-modified graphitic carbon nitride derivative yellow-green light material, characterized in that... The raw materials required to prepare this material are melamine and 6-(4-(9) H- Carbazole-9-yl)phenyl)-1,3,5-triazine-2,4-diamine is prepared by a high-temperature solid-state reaction method, including the following steps: reacting melamine with 6-(4-(9-yl)phenyl)-1,3,5-triazine-2,4-diamine. H- Carbazole-9-yl)phenyl)-1,3,5-triazine-2,4-diamine was mixed and ground evenly, and the evenly ground mixture was polymerized at 450 degrees Celsius for 2 hours under nitrogen protection.

Citation Information

Patent Citations

  • Preparation method of green fluorescent carbon nitride powder

    CN106833609A

  • Graphite-phase carbon nitride-based green light material preparation method

    CN110540836A