A high-entropy alloy hydrotalcite oxide composite material, a preparation method and application thereof
By loading high-entropy alloys onto a hydrotalcite oxide support, a high-entropy alloy-based hydrotalcite oxide composite material was prepared, which solved the problems of easy catalyst deactivation and low selectivity in the dry reforming reaction of methane and achieved a high-efficiency catalytic effect under mild conditions.
Patent Information
- Application Number
- CN202410664833.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-27
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-05-27
AI Technical Summary
Existing catalysts suffer from low selectivity and severe coking leading to catalyst deactivation in methane dry reforming reactions. Furthermore, traditional thermocatalytic reactions require high temperatures, making it difficult to improve reaction yields under mild conditions.
High-entropy alloy-based hydrotalcite oxide composite material was used as a catalyst. By loading high-entropy alloy onto the hydrotalcite oxide support, the reaction temperature was increased under moderate light irradiation by utilizing the nano-heating function of the high-entropy alloy. The adsorption capacity of CO₂ and CH₄ was improved by adjusting the material ratio of Ti⁴⁺, Li⁺, and Al³⁺.
Ultra-high yield and selectivity of methane dry reforming reaction were achieved without external heating. The catalyst can work effectively at a surface reaction temperature of 560℃, solving the problem of deactivation of traditional catalysts at high temperatures.
Smart Images

Figure HDA0004860782790000011 
Figure HDA0004860782790000012 
Figure HDA0004860782790000021
Abstract
Description
Technical Field
[0001] This invention belongs to the field of catalyst preparation technology, specifically relating to a high-entropy alloy-type hydrotalcite oxide composite material, its preparation method, and its application. Background Technology
[0002] Layered bimetallic hydroxides (LDHs) are two-dimensional materials, typically consisting of positively charged layers (metal ions) and anionic layers, with water between the layers. Their unique structure, stability, ease of synthesis, and low cost have attracted interest in the field of catalysis.
[0003] High-entropy alloys typically contain five or more elements (in equimolar or near-equimolar ratios) and have attracted increasing attention in recent years due to their unique properties in various applications. They exhibit excellent C=O bond breaking ability in CO2 hydrogenation and CH dissociation ability in propane dehydrogenation. Furthermore, the incomplete filling of d-states in the composition allows high-entropy alloys to collect photons across the entire solar spectrum through interband excitation, thus providing superior photothermal conversion efficiency.
[0004] With the continued growth of global energy demand leading to increased consumption of fossil fuels and carbon dioxide (CO2) emissions, addressing carbon emission issues through CO2 capture, utilization, and storage is of great significance. Dry methane reforming (DRM, CH4 + CO2 = 2CO + 2H2) is an environmentally friendly and economical strategy for converting greenhouse gases CO2 and CH4 into syngas (H2 and CO) for the synthesis of valuable chemicals and value-added liquid fuels, offering a promising strategy for addressing energy shortages. However, the DRM reaction is a highly endothermic reaction (ΔH... 298 =247kJ mol -1 Traditional thermocatalytic reactions typically require high temperatures (>700℃) and suffer from low selectivity and severe coking leading to catalyst deactivation. Therefore, designing a novel catalyst that can significantly improve the yield of methane dry reforming under mild conditions is a pressing issue. Summary of the Invention
[0005] To overcome the problems of low selectivity and severe coking leading to catalyst deactivation in the DRM reaction in the prior art, the purpose of this invention is to provide a high-entropy alloy-type hydrotalcite oxide composite material, its preparation method, and its application.
[0006] To achieve the above objectives, the technical solution adopted by the present invention is as follows:
[0007] A method for preparing a high-entropy alloy-type hydrotalcite oxide composite material includes the following steps:
[0008] TiCl4, LiCl and AlCl3·6H2O were mixed evenly, the pH was adjusted to 7-8, and then reacted at 75-110℃ for 24-48h. After drying, a hydrotalcite-like material containing titanium, lithium and aluminum was obtained.
[0009] A layered double hydroxide-like material containing titanium, lithium, and aluminum was added to deionized water and stirred until homogeneous. Then, a solution containing a metal precursor was added and stirred until homogeneous. After removing the deionized water, the mixture was calcined under a protective atmosphere to obtain a high-entropy alloy layered double hydroxide oxide composite material.
[0010] Furthermore, the pH value was adjusted to 7-8 using a mixed solution of KOH and Na2CO3 with a molar ratio of 2.25:1.
[0011] Furthermore, the molar ratio of TiCl4, LiCl and AlCl3·6H2O is (1-2):3:(2-6).
[0012] Furthermore, the ratio of the titanium-lithium-aluminum-based hydrotalcite material to deionized water is 230-340 mg: 40 mL.
[0013] Furthermore, the ratio of the titanium-lithium-aluminum-based hydrotalcite-like material to the metal precursor solution is 230-340 mg: 5 mL;
[0014] The protective atmosphere, by volume percentage, comprises 5% H2 and 95% Ar.
[0015] Furthermore, the calcination temperature is 300-500℃, and the time is 2-4 hours.
[0016] Furthermore, at 5-10℃ min -1 The heating rate is increased to 300-500℃.
[0017] Furthermore, the metal precursor solution is a mixture of 10 mmol / L copper nitrate hexahydrate solution, 10 mmol / L nickel nitrate hexahydrate solution, 10 mmol / L ruthenium trichloride trihydrate solution, 10 mmol / L rhodium trichloride trihydrate solution, and 10 mmol / L sodium chloropalladate solution in a volume ratio of 1:1:1:1:1; or
[0018] The metal precursor solution is a mixture of 10 mmol / L cobalt nitrate hexahydrate, 10 mmol / L nickel nitrate hexahydrate, 10 mmol / L ruthenium trichloride trihydrate, 10 mmol / L rhodium trichloride trihydrate, and 10 mmol / L sodium chloropalladate solution in a volume ratio of 1:1:1:1:1; or
[0019] The metal precursor solution was a mixture of 10 mmol / L chloroauric acid solution, 10 mmol / L nickel nitrate hexahydrate solution, 10 mmol / L ruthenium trichloride trihydrate solution, 10 mmol / L rhodium trichloride trihydrate solution and 10 mmol / L sodium chloropalladate solution in a volume ratio of 1:1:1:1:1:1.
[0020] A high-entropy alloy-type hydrotalcite oxide composite material.
[0021] Application of a high-entropy alloy-type hydrotalcite oxide composite material in photocatalytic dry reforming of methane.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] This invention utilizes a hydrotalcite-like oxide to support a high-entropy alloy. While calcining the hydrotalcite-like material to form a hydrotalcite-like oxide, a high-entropy alloy is synthesized and loaded onto a hydrotalcite oxide support, providing a novel preparation method for high-entropy alloy-hydrotalcite oxide composites. Using the hydrotalcite oxide as a support enhances the adsorption capacity for CO2 and CH4, while the high-entropy alloy serves as the active component, providing heating functionality and acting as a "nanoheater," enabling the surface reaction temperature to reach 560°C under moderate light irradiation without external heating. This catalyst can be applied to photocatalytic dry reforming of methane. This invention provides a novel method for photocatalytic dry reforming of methane, achieving extremely high yields and selectivity.
[0024] Furthermore, the Ti in this invention is used 4+ Li + Al 3+ The molar ratio of these substances increases the adsorption of CO2 and CH4.
[0025] Furthermore, the synthesis of high-entropy alloys requires a high temperature of 400°C under hydrogen conditions (hydrogen was chosen to reduce the metal salt solution to metal). Simultaneously, the calcination of LDHs to LDOs also requires temperatures above 300°C. Therefore, the synthesis of high-entropy alloys is carried out simultaneously with the calcination of LDHs to LDOs under a 5% H2 / 95% Ar atmosphere at 400°C. Since H2 reduction at high temperatures is relatively dangerous, 5% H2 is sufficient.
[0026] Furthermore, loading pure TiLiAl-LDOs and TiLiAl-LDOs with single metals such as Cu, Ni, Ru, Rh, and Pd did not yield good reaction results. Only after loading with high-entropy alloys did ultra-high yields and excellent selectivity be achieved. This indicates that the integration of hydrotalcite oxides and high-entropy alloys plays a crucial role. Moreover, under 4W light intensity, pure TiLiAl-LDOs produced a temperature of 430℃, while TiLiAl-LDOs / Rh, after loading with a single metal Rh, achieved a temperature of 490℃, and Ti1Li3Al6-LDOs / HEAs achieved a high temperature of 560℃. This demonstrates that the high-entropy alloys act as "nanotherapeutic heaters."
[0027] Furthermore, Ni, Rh, Ru, and Pd are considered the primary active metals in this invention because they have previously been shown to have the potential for CH cleavage, while the late 3d transition metal Cu is used to promote CO2 reduction. Simultaneously, TiLiAl-LDOs materials with moderately basic sites are screened as supports to enhance CO2 adsorption and dissociation. Needless to say, the high-entropy alloy can also absorb a broad spectrum of light and act as a "nanoheater," rapidly raising the local temperature to 560°C. Attached Figure Description
[0028] Figure 1 This is a schematic diagram of the synthesis of the present invention;
[0029] Figure 2 Here is a SEM image of Ti1Li3Al6-LDHs in this invention;
[0030] Figure 3 This is a TEM image of Ti1Li3Al6-LDHs in this invention;
[0031] Figure 4 The XRD patterns of Ti1Li3Al6-LDHs at different calcination temperatures in this invention are shown below.
[0032] Figure 5 This is a comparison chart of the performance of Ti1Li3Al6-LDHs at different calcination temperatures in this invention.
[0033] Figure 6 The images are STEM images of the high-entropy alloy particles in Ti1Li3Al6-CuNiRuRhPd-HEAs in this invention; where (a) is a STEM image and (b) is an enlarged view of the area within the box in (a).
[0034] Figure 7 The XRD patterns of the high-entropy alloys in Ti1Li3Al6-LDOs and Ti1Li3Al6-CuNiRuRhPd-HEAs in this invention are shown.
[0035] Figure 8 This is a comparison chart of the performance tests of Ti1Li3Al6-LDHs loaded with a single metal and CuNiRuRhPd high-entropy alloy particles in this invention.
[0036] Figure 9 This is a graph showing the entropy value determination of the high-entropy alloy in Ti1Li3Al6-CuNiRuRhPd-HEAs in this invention;
[0037] Figure 10 This is a comparison of the temperatures generated by Ti1Li3Al6-LDOs, Ti1Li3Al6-LDOs / Rh, and Ti1Li3Al6-CuNiRuRhPd-HEAs under a light intensity of 4W in this invention. Detailed Implementation
[0038] To facilitate understanding of the present invention, a more complete description will be given below with reference to the accompanying drawings. Preferred embodiments of the invention are shown in the drawings. However, the invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided to provide a thorough and complete understanding of the disclosure of the invention.
[0039] Hydrotalcites (LDHs) are a class of anionic compounds with a special layered structure, composed of metal hydroxides. Their chemical structural formula is represented as [M]. 1-x Ⅱ ·M x Ⅲ ·(OH)2] z+ [A n- ]z / n·mH2O, where M 2+ Represents Cu 2+ Ca 2+ Co 2+ Mg 2+ Zn 2+ Ni 2+ Divalent metal cations, M 3+ Representing Al 3+ V 3+ Cr 3+ Fe 3+ Mn 3+ Trivalent metal cations, A n- CO3 2- NO 3- PO4 3- SO4 2- Cl - I - The anions are typically between 0.17 and 0.34. This invention relates to a hydrotalcite-like material.
[0040] The present invention discloses a method for preparing a high-entropy alloy-type hydrotalcite oxide composite material, comprising the following steps:
[0041] First, TiCl4, LiCl, and AlCl3·6H2O were added to a flask and stirred for 1 hour. Then, while stirring, a mixed solution of KOH and Na2CO3 (molar ratio KOH:Na2CO3 = 2.25:1) was added dropwise until the pH value was between 7 and 8. Stirring was continued for another hour. The reaction solution was then transferred to a water bath and reacted at 75-110℃ for 24-48 hours. After the reaction, the mixture was filtered and washed several times with deionized water and ethanol. It was then dried in a vacuum drying oven at 60℃ for 10-12 hours to obtain a layered double hydroxide material containing titanium lithium aluminum, denoted as TiLiAl-LDHs. The molar ratio of TiCl4, LiCl, and AlCl3·6H2O was (1-2):3:(2-6).
[0042] Add 230-340 mg TiLiAl-LDHs to 40 mL of deionized water and stir vigorously for 0.5 hours. Then add 5 mL of metal precursor solution and stir at room temperature for 1 hour. Volatilize at 80 °C for 10-12 hours until all deionized water is removed. Transfer the solution to a mortar and grind. Calcine the resulting sample at 300-500 °C for 2-4 hours (heating rate 5-10 °C / min) under a 5% (v / v) H₂ / 95% Ar atmosphere. -1 ), thus obtaining a high-entropy alloy-type hydrotalcite oxide composite material.
[0043] The metal precursor solution is a mixture of 10 mmol / L copper nitrate hexahydrate, 10 mmol / L nickel nitrate hexahydrate, 10 mmol / L ruthenium trichloride trihydrate, 10 mmol / L rhodium trichloride trihydrate, and 10 mmol / L sodium chloropalladate solution in a volume ratio of 1:1:1:1:1; or
[0044] The metal precursor solution is a mixture of 10 mmol / L cobalt nitrate hexahydrate, 10 mmol / L nickel nitrate hexahydrate, 10 mmol / L ruthenium trichloride trihydrate, 10 mmol / L rhodium trichloride trihydrate, and 10 mmol / L sodium chloropalladate solution in a volume ratio of 1:1:1:1:1; or
[0045] The metal precursor solution was a mixture of 10 mmol / L chloroauric acid solution, 10 mmol / L nickel nitrate hexahydrate solution, 10 mmol / L ruthenium trichloride trihydrate solution, 10 mmol / L rhodium trichloride trihydrate solution and 10 mmol / L sodium chloropalladate solution in a volume ratio of 1:1:1:1:1:1.
[0046] In this invention, a high-entropy alloy refers to an alloy with an entropy value greater than 1.5R.
[0047] The following are specific examples.
[0048] Example 1
[0049] (1) First, mix TiCl4 (0.925 mL), LiCl (1.05975 g), and AlCl3·6H2O (4.0225 g) in a flask. 4+ Li + Al 3+ The molar ratio of the substances was 1:3:2. After mixing, the mixture was stirred for 1 hour. Then, while stirring, a mixed solution of KOH and Na2CO3 (molar ratio KOH:Na2CO3 = 2.25:1) was added dropwise until the pH value reached 7.5. Stirring was continued for another hour. The reaction solution was then transferred to a water bath and reacted at 75°C for 48 hours. After the reaction, the solution was filtered, washed several times with deionized water and ethanol, and dried in a vacuum drying oven at 60°C for 12 hours to obtain Ti1Li3Al2-LDHs.
[0050] (2) 340 mg of Ti1Li3Al2-LDHs was added to 40 mL of deionized water and stirred vigorously for 0.5 hours. Then, five metal precursor solutions were added: copper nitrate hexahydrate solution (1 mL, containing 2.91 mg of copper nitrate hexahydrate), nickel nitrate hexahydrate solution (1 mL, containing 2.91 mg of nickel nitrate hexahydrate), ruthenium trichloride trihydrate solution (1 mL, containing 2.07 mg of ruthenium trichloride trihydrate), rhodium trichloride trihydrate solution (1 mL, containing 2.63 mg of rhodium trichloride trihydrate), and sodium chloropalladium solution (1 mL, containing 2.94 mg of sodium chloropalladium). After stirring at room temperature for 1 hour, the solution was evaporated at 80 °C for 10-12 hours until the deionized water was completely removed. The solution was then transferred to a mortar and ground. The resulting sample was calcined at 400 °C for 4 hours (heating rate 5 °C / min) under a 5% H2 / 95% Ar atmosphere. -1 A high-entropy alloy-like hydrotalcite oxide composite material, denoted as Ti1Li3Al2-LDOs / CuNiRuRhPd-HEAs, was obtained. Its high-entropy alloy configuration entropy value is 1.53R, which proves its high-entropy characteristics.
[0051] Methane dry reforming performance test:
[0052] The DRM reaction was carried out in a continuous flow fixed-bed reactor (Beijing Pofilai Technology Co., Ltd.). In the test, 2 mg of the Ti1Li3Al2-LDOs / CuNiRuRhPd-HEAs prepared in Example 1 was uniformly dispersed on glass fiber filter paper with a diameter of 3 cm. After the sample was placed in the sealed reactor, the reaction gas (10% CH4 / 10% CO2 / 80% Ar) was introduced at a rate of 10 mL / min. -1 The feed gas was introduced into the reactor at a flow rate of [missing information]. A 300W xenon lamp (PLS-SXE300, Perfect Light) was used as the light source to drive the DRM reaction. After the feed gas reached equilibrium adsorption, the gaseous products were detected by a gas chromatograph (GC97902Ⅱ, Fuli), equipped with two flame ionization detectors (FID) and one thermal conductivity detector (TCD) to evaluate the products.
[0053] The results showed that the yield of H2 / CO was (28.11 / 29.58 mol) -1 g metal -1 h -1 The selectivity was 0.95.
[0054] Example 2
[0055] (1) First, mix TiCl4 (0.555 mL), LiCl (0.635 g), and AlCl3·6H2O (7.245 g) in a flask. 4+ Li + Al 3+ The molar ratio of the substances was 1:3:6. After mixing, the mixture was stirred for 1 hour. Then, while stirring, a mixed solution of KOH and Na₂CO₃ (KOH:Na₂CO₃ = 2.25:1) was added dropwise until the pH reached 7.5. Stirring continued for another hour. The reaction solution was then transferred to a water bath and reacted at 75°C for 48 hours. After the reaction, the mixture was filtered, washed several times with deionized water and ethanol, and dried in a vacuum drying oven at 60°C for 10-12 hours to obtain Ti₁Li₃Al₆-LDHs.
[0056] See Figure 2 As can be seen, the synthesized hydrotalcite has a distinct layered structure with a size of about 100 nm.
[0057] See Figure 3 As can be seen, the synthesized hydrotalcite has a distinct layered structure.
[0058] See Figure 4 ,from Figure 4 It can be seen that LDHs can only be calcined into LDOs at temperatures above 300℃, which also corresponds to... Figure 5 Differences in performance testing.
[0059] See Figure 5 ,from Figure 5 As can be seen, the reason why there is a significant improvement above 300℃ is that LDHs are calcined into LDOs above this temperature.
[0060] (2) 340 mg Ti1Li3Al6-LDHs was added to 40 mL of deionized water and stirred vigorously for 0.5 hours. Then, five metal precursor solutions were added: copper nitrate hexahydrate (1 mL, containing 2.91 mg copper nitrate hexahydrate), nickel nitrate hexahydrate (1 mL, containing 2.91 mg nickel nitrate hexahydrate), ruthenium trichloride trihydrate (1 mL, containing 2.07 mg ruthenium trichloride trihydrate), rhodium trichloride trihydrate (1 mL, containing 2.63 mg rhodium trichloride trihydrate), and sodium chloropalladium (1 mL, containing 2.94 mg sodium chloropalladium). After stirring at room temperature for 1 hour, the solution was evaporated at 80 °C for 10-12 hours until all deionized water was removed. The solution was then transferred to a mortar and ground. The resulting sample was calcined at 400 °C for 4 hours (heating rate 5 °C / min) under a 5% H2 / 95% Ar atmosphere. -1 A high-entropy alloy-like hydrotalcite oxide composite material, denoted as Ti1Li3Al6-LDOs / CuNiRuRhPd-HEAs, was obtained. Its high-entropy alloy configuration entropy value is 1.56R, which proves its high-entropy characteristics.
[0061] See Figure 6 In (a) and (b), it can be seen that the lattice fringes correspond to Figure 7 The (111) crystal plane.
[0062] See Figure 7 As can be seen, the peak of the (111) crystal plane represents the formation of high-entropy alloys, and there are no peaks of the five metals Cu, Ni, Ru, Rh, Pd in the figure.
[0063] See Figure 8 It can be seen that the performance of a single metal under load is generally poor, so the good performance is due to the integration effect of the high-entropy alloy.
[0064] See Figure 9 As can be seen, the atomic percentages of the five metal elements obtained by inductively coupled plasma atomic emission spectrometry (ICP-AES) yielded a configuration entropy value greater than 1.5R (where R is the universal gas constant), proving their high entropy characteristics.
[0065] See Figure 10It can be seen that, based on the temperature comparison of Ti1Li3Al6-LDOs, Ti1Li3Al6-LDOs / Rh, and Ti1Li3Al6-LDOs / CuNiRuRhPd-HEAs under illumination, it is observed that due to the integration effect of high-entropy alloys, a high temperature of 560℃ can be generated, which is beneficial to the reaction.
[0066] Methane dry reforming performance test:
[0067] The DRM reaction was carried out in a continuous flow fixed-bed reactor (Beijing Pofilai Technology Co., Ltd.). In the test, 2 mg of the Ti1Li3Al6-LDOs / CuNiRuRhPd-HEAs prepared in Example 2 was uniformly dispersed on glass fiber filter paper with a diameter of 3 cm. After the sample was placed in the sealed reactor, the reaction gas (10% CH4 / 10% CO2 / 80% Ar) was introduced at a rate of 10 mL / min. -1 The feed gas was introduced into the reactor at a flow rate of [missing information]. A 300W xenon lamp (PLS-SXE300, Perfect Light) was used as the light source to drive the DRM reaction. After the feed gas reached equilibrium adsorption, the gaseous products were detected by a gas chromatograph (GC97902Ⅱ, Fuli), equipped with two flame ionization detectors (FID) and one thermal conductivity detector (TCD) to evaluate the products.
[0068] The results showed that the yield of H2 / CO was (45.82 / 46.59 mol) -1 g metal -1 h -1 The selectivity was 0.98.
[0069] Example 3
[0070] (1) First, mix TiCl4 (0.555 mL), LiCl (0.635 g), and AlCl3·6H2O (7.245 g) in a flask. 4+ Li + Al 3+ The molar ratio of the substances was 1:3:6. After mixing, the mixture was stirred for 1 hour. Then, while stirring, a mixed solution of KOH and Na₂CO₃ (KOH:Na₂CO₃ = 2.25:1) was added dropwise until the pH reached 7.5. Stirring continued for another hour. The reaction solution was then transferred to a water bath and reacted at 75°C for 48 hours. After the reaction, the mixture was filtered, washed several times with deionized water and ethanol, and dried in a vacuum drying oven at 60°C for 10-12 hours to obtain Ti₁Li₃Al₆-LDHs.
[0071] (2) 340 mg Ti1Li3Al6-LDHs was added to 40 mL of deionized water and stirred vigorously for 0.5 hours. Then, five metal precursor solutions were added: cobalt nitrate hexahydrate (1 mL, containing 2.91 mg cobalt nitrate hexahydrate), nickel nitrate hexahydrate (1 mL, containing 2.91 mg nickel nitrate hexahydrate), ruthenium trichloride trihydrate (1 mL, containing 2.07 mg ruthenium trichloride trihydrate), rhodium trichloride trihydrate (1 mL, containing 2.63 mg rhodium trichloride trihydrate), and sodium chloropalladium (1 mL, containing 2.94 mg sodium chloropalladium). After stirring at room temperature for 1 hour, the solution was evaporated at 80 °C for 10-12 hours until all deionized water was removed. The solution was then transferred to a mortar and ground. The resulting sample was calcined at 400 °C for 4 hours (heating rate 5 °C / min) under a 5% H2 / 95% Ar atmosphere. -1 A high-entropy alloy-like hydrotalcite oxide composite material, denoted as Ti1Li3Al6-LDOs / CoNiRuRhPd-HEAs, was obtained. Its high-entropy alloy configuration entropy value is 1.53R, which proves its high-entropy characteristics.
[0072] Methane dry reforming performance test:
[0073] The DRM reaction was carried out in a continuous flow fixed-bed reactor (Beijing Pofilai Technology Co., Ltd.). In the test, 2 mg of the Ti1Li3Al6-LDOs / CoNiRuRhPd-HEAs prepared in Example 3 was uniformly dispersed on glass fiber filter paper with a diameter of 3 cm. After the sample was placed in the sealed reactor, the reaction gas (10% CH4 / 10% CO2 / 80% Ar) was introduced at a rate of 10 mL / min. -1 The feed gas was introduced into the reactor at a flow rate of [missing information]. A 300W xenon lamp (PLS-SXE300, Perfect Light) was used as the light source to drive the DRM reaction. After the feed gas reached equilibrium adsorption, the gaseous products were detected by a gas chromatograph (GC97902Ⅱ, Fuli), equipped with two flame ionization detectors (FID) and one thermal conductivity detector (TCD) to evaluate the products.
[0074] The results showed that the yield of H2 / CO was (38.57 / 42.02 mol) -1 g metal -1 h -1 The selectivity was 0.92.
[0075] Example 4
[0076] (1) First, mix TiCl4 (0.555 mL), LiCl (0.635 g), and AlCl3·6H2O (7.245 g) in a flask. 4+ Li+ Al 3+ The molar ratio of the substances was 1:3:6. After mixing, the mixture was stirred for 1 hour. Then, while stirring, a mixed solution of KOH and Na₂CO₃ (KOH:Na₂CO₃ = 2.25:1) was added dropwise until the pH reached 7.5. Stirring continued for another hour. The reaction solution was then transferred to a water bath and reacted at 75°C for 48 hours. After the reaction, the mixture was filtered, washed several times with deionized water and ethanol, and dried in a vacuum drying oven at 60°C for 10-12 hours to obtain Ti₁Li₃Al₆-LDHs.
[0077] (2) 340 mg of Ti1Li3Al6-LDHs was added to 40 mL of deionized water and stirred vigorously for 0.5 hours. Then, five metal precursor solutions were added: chloroauric acid solution (1 mL, containing 3.4 mg of chloroauric acid), nickel nitrate hexahydrate (1 mL, containing 2.91 mg of nickel nitrate hexahydrate), ruthenium trichloride trihydrate (1 mL, containing 2.07 mg of ruthenium trichloride trihydrate), rhodium trichloride trihydrate (1 mL, containing 2.63 mg of rhodium trichloride trihydrate), and sodium chloropalladium (1 mL, containing 2.94 mg of sodium chloropalladium). After stirring at room temperature for 1 hour, the solution was evaporated at 80 °C for 10-12 hours until all deionized water was removed. The solution was then transferred to a mortar and ground. The resulting sample was calcined at 400 °C for 4 hours (heating rate 5 °C / min) under a 5% H2 / 95% Ar atmosphere. -1 A high-entropy alloy-like hydrotalcite oxide composite material, denoted as Ti1Li3Al6-LDOs / AuNiRuRhPd-HEAs, was obtained. Its high-entropy alloy configuration entropy value is 1.52R, which proves its high-entropy characteristics.
[0078] Methane dry reforming performance test:
[0079] The DRM reaction was carried out in a continuous flow fixed-bed reactor (Beijing Pofilai Technology Co., Ltd.). In the test, 2 mg of the Ti1Li3Al6-LDOs / AuNiRuRhPd-HEAs prepared in Example 4 was uniformly dispersed on glass fiber filter paper with a diameter of 3 cm. After the sample was placed in the sealed reactor, the reaction gas (10% CH4 / 10% CO2 / 80% Ar) was introduced at a rate of 10 mL / min. -1 The feed gas was introduced into the reactor at a flow rate of [missing information]. A 300W xenon lamp (PLS-SXE300, Perfect Light) was used as the light source to drive the DRM reaction. After the feed gas reached equilibrium adsorption, the gaseous products were detected by a gas chromatograph (GC97902Ⅱ, Fuli), equipped with two flame ionization detectors (FID) and one thermal conductivity detector (TCD) to evaluate the products.
[0080] The results showed that the yields of H2 / CO were (38.92 / 39.93 mol)-1 g metal -1 h -1 The selectivity was 0.97.
[0081] Example 5
[0082] (1) First, take CaCl2 (0.925g), LiCl (1.05975g), and AlCl3·6H2O (4.0225g) and mix them in a flask. 2+ Li + Al 3+ The molar ratio of the substances was 1:3:2. After mixing, the mixture was stirred for 1 hour. Then, while stirring, a mixed solution of KOH and Na₂CO₃ (molar ratio KOH:Na₂CO₃ = 2.25:1) was added dropwise until the pH reached 7.5. Stirring continued for another hour. The reaction solution was then transferred to a water bath and reacted at 75°C for 48 hours. After the reaction, the solution was filtered, washed several times with deionized water and ethanol, and dried in a vacuum drying oven at 60°C for 12 hours to obtain Ca₁Li₃Al₂-LDHs.
[0083] (2) 340 mg of Ca1Li3Al2-LDHs was added to 40 mL of deionized water and stirred vigorously for 0.5 hours. Then, five metal precursor solutions were added: copper nitrate hexahydrate solution (1 mL, containing 2.91 mg of copper nitrate hexahydrate), nickel nitrate hexahydrate solution (1 mL, containing 2.91 mg of nickel nitrate hexahydrate), ruthenium trichloride trihydrate solution (1 mL, containing 2.07 mg of ruthenium trichloride trihydrate), rhodium trichloride trihydrate solution (1 mL, containing 2.63 mg of rhodium trichloride trihydrate), and sodium chloropalladium solution (1 mL, containing 2.94 mg of sodium chloropalladium). After stirring at room temperature for 1 hour, the solution was evaporated at 80 °C for 10-12 hours until all deionized water was removed. The solution was then transferred to a mortar and ground. The resulting sample was calcined at 400 °C for 4 hours (heating rate 5 °C / min) under a 5% H2 / 95% Ar atmosphere. -1 A high-entropy alloy-like hydrotalcite oxide composite material, denoted as Ca1Li3Al2-LDOs / CuNiRuRhPd-HEAs, was obtained. Its high-entropy alloy configuration entropy value is 1.55R, which proves its high-entropy characteristics.
[0084] Methane dry reforming performance test:
[0085] The DRM reaction was carried out in a continuous flow fixed-bed reactor (Beijing Pofilai Technology Co., Ltd.). In the test, 2 mg of the Ca1Li3Al2-LDOs / CuNiRuRhPd-HEAs prepared in Example 5 was uniformly dispersed on glass fiber filter paper with a diameter of 3 cm. After the sample was placed in the sealed reactor, the reaction gas (10% CH4 / 10% CO2 / 80% Ar) was introduced at a rate of 10 mL / min. -1 The feed gas was introduced into the reactor at a flow rate of [missing information]. A 300W xenon lamp (PLS-SXE300, Perfect Light) was used as the light source to drive the DRM reaction. After the feed gas reached equilibrium adsorption, the gaseous products were detected by a gas chromatograph (GC97902Ⅱ, Fuli), equipped with two flame ionization detectors (FID) and one thermal conductivity detector (TCD) to evaluate the products.
[0086] The results showed that the yields of H2 / CO were (32.5 / 33.48 mol) -1 g metal -1 h -1 The selectivity was 0.97.
[0087] Example 6
[0088] (1) First, mix TiCl4 (0.925 mL), LiCl, and AlCl3·6H2O into a flask. 4+ Li + Al 3+ The molar ratio of the substances was 2:3:2. After mixing, the mixture was stirred for 1 hour. Then, while stirring, a mixed solution of KOH and Na₂CO₃ (molar ratio KOH:Na₂CO₃ = 2.25:1) was added dropwise until the pH value reached 7, and stirring was continued for another hour. The above reaction solution was transferred to a water bath and reacted at 110℃ for 24 hours. After the reaction, the mixture was filtered, washed several times with deionized water and ethanol, and dried in a vacuum drying oven at 60℃ for 10 hours to obtain a hydrotalcite-like material containing titanium-lithium-aluminum.
[0089] (2) 230 mg of a layered double hydroxide containing titanium-lithium-aluminum was added to 40 mL of deionized water and stirred vigorously for 0.5 hours. Then, five metal precursor solutions were added: copper nitrate hexahydrate solution (1 mL, containing 2.91 mg of copper nitrate hexahydrate), nickel nitrate hexahydrate solution (1 mL, containing 2.91 mg of nickel nitrate hexahydrate), ruthenium trichloride trihydrate solution (1 mL, containing 2.07 mg of ruthenium trichloride trihydrate), rhodium trichloride trihydrate solution (1 mL, containing 2.63 mg of rhodium trichloride trihydrate), and sodium chloropalladium solution (1 mL, containing 2.94 mg of sodium chloropalladium). After stirring at room temperature for 1 hour, the solution was evaporated at 80 °C for 10 hours until all deionized water was removed. The solution was then transferred to a mortar and ground. The resulting sample was calcined at 300 °C for 4 hours (heating rate 10 °C / min) under a 5% H2 / 95% Ar atmosphere. -1 A high-entropy alloy-like hydrotalcite oxide composite material was obtained, with a high-entropy alloy configuration entropy value of 1.54R, which proves its high-entropy characteristics.
[0090] Example 7
[0091] (1) First, mix TiCl4 (0.925 mL), LiCl, and AlCl3·6H2O into a flask. 4+ Li + Al 3+ The molar ratio of the substances was 2:3:6. After mixing, the mixture was stirred for 1 hour. Then, while stirring, a mixed solution of KOH and Na₂CO₃ (molar ratio KOH:Na₂CO₃ = 2.25:1) was added dropwise until the pH reached 7. Stirring continued for another hour. The reaction solution was then transferred to a water bath and reacted at 75°C for 48 hours. After the reaction, the mixture was filtered, washed several times with deionized water and ethanol, and dried in a vacuum drying oven at 60°C for 11 hours to obtain a hydrotalcite-like material containing titanium, lithium, and aluminum.
[0092] (2) 300 mg of Ti1Li3Al2-LDHs was added to 40 mL of deionized water and stirred vigorously for 0.5 hours. Then, five metal precursor solutions were added: copper nitrate hexahydrate solution (1 mL, containing 2.91 mg of copper nitrate hexahydrate), nickel nitrate hexahydrate solution (1 mL, containing 2.91 mg of nickel nitrate hexahydrate), ruthenium trichloride trihydrate solution (1 mL, containing 2.07 mg of ruthenium trichloride trihydrate), rhodium trichloride trihydrate solution (1 mL, containing 2.63 mg of rhodium trichloride trihydrate), and sodium chloropalladium solution (1 mL, containing 2.94 mg of sodium chloropalladium). After stirring at room temperature for 1 hour, the solution was evaporated at 80 °C for 11 hours until all deionized water was removed. The solution was then transferred to a mortar and ground. The resulting sample was calcined at 500 °C for 2 hours (heating rate 7 °C / min) under a 5% H2 / 95% Ar atmosphere. -1A high-entropy alloy-like hydrotalcite oxide composite material was obtained, with a high-entropy alloy configuration entropy value of 1.56R, which proves its high-entropy characteristics.
[0093] Example 8
[0094] (1) First, mix TiCl4 (0.925 mL), LiCl, and AlCl3·6H2O into a flask. 4+ Li + Al 3+ The molar ratio of the substances was 2:3:4. After mixing, the mixture was stirred for 1 hour. Then, while stirring, a mixed solution of KOH and Na2CO3 (molar ratio KOH:Na2CO3 = 2.25:1) was added dropwise until the pH value reached 7.5, and stirring was continued for another hour. The above reaction solution was transferred to a water bath and reacted at 80°C for 30 hours. After the reaction, the mixture was filtered, washed several times with deionized water and ethanol, and dried in a vacuum drying oven at 60°C for 12 hours to obtain a hydrotalcite-like material containing titanium, lithium, and aluminum.
[0095] (2) 270 mg of Ti1Li3Al2-LDHs was added to 40 mL of deionized water and stirred vigorously for 0.5 hours. Then, five metal precursor solutions were added: copper nitrate hexahydrate solution (1 mL, containing 2.91 mg of copper nitrate hexahydrate), nickel nitrate hexahydrate solution (1 mL, containing 2.91 mg of nickel nitrate hexahydrate), ruthenium trichloride trihydrate solution (1 mL, containing 2.07 mg of ruthenium trichloride trihydrate), rhodium trichloride trihydrate solution (1 mL, containing 2.63 mg of rhodium trichloride trihydrate), and sodium chloropalladium solution (1 mL, containing 2.94 mg of sodium chloropalladium). After stirring at room temperature for 1 hour, the solution was evaporated at 80 °C for 12 hours until all deionized water was removed. The solution was then transferred to a mortar and ground. The resulting sample was calcined at 350 °C for 3 hours (heating rate 6 °C / min) under a 5% H2 / 95% Ar atmosphere. -1 A high-entropy alloy-like hydrotalcite oxide composite material was obtained, with a high-entropy alloy configuration entropy value of 1.52R, which proves its high-entropy characteristics.
[0096] Example 9
[0097] (1) First, mix TiCl4 (0.925 mL), LiCl, and AlCl3·6H2O into a flask. 4+ Li + Al 3+The molar ratio of the substances was 1:3:5. After mixing, the mixture was stirred for 1 hour. Then, while stirring, a mixed solution of KOH and Na₂CO₃ (molar ratio KOH:Na₂CO₃ = 2.25:1) was added dropwise until the pH value reached 8, and stirring was continued for another hour. The above reaction solution was transferred to a water bath and reacted at 100°C for 26 hours. After the reaction, the mixture was filtered, washed several times with deionized water and ethanol, and dried in a vacuum drying oven at 60°C for 10 hours to obtain a hydrotalcite-like material containing titanium-lithium-aluminum.
[0098] (2) 320 mg of Ti1Li3Al2-LDHs was added to 40 mL of deionized water and stirred vigorously for 0.5 hours. Then, five metal precursor solutions were added: copper nitrate hexahydrate solution (1 mL, containing 2.91 mg of copper nitrate hexahydrate), nickel nitrate hexahydrate solution (1 mL, containing 2.91 mg of nickel nitrate hexahydrate), ruthenium trichloride trihydrate solution (1 mL, containing 2.07 mg of ruthenium trichloride trihydrate), rhodium trichloride trihydrate solution (1 mL, containing 2.63 mg of rhodium trichloride trihydrate), and sodium chloropalladium solution (1 mL, containing 2.94 mg of sodium chloropalladium). After stirring at room temperature for 1 hour, the solution was evaporated at 80 °C for 10 hours until all deionized water was removed. The solution was then transferred to a mortar and ground. The resulting sample was calcined at 460 °C for 2 hours (heating rate 8 °C / min) under a 5% H2 / 95% Ar atmosphere. -1 A high-entropy alloy-like hydrotalcite oxide composite material was obtained, with a high-entropy alloy configuration entropy value of 1.54R, which proves its high-entropy characteristics.
[0099] Comparative Example 1
[0100] (1) First, mix LiCl (0.635g) and AlCl3·6H2O (7.245g) in a flask, then... + Al 3+ The molar ratio of the substances was 1:2. After mixing, the mixture was stirred for 1 hour. Then, while stirring, a mixed solution of KOH and Na₂CO₃ (KOH:Na₂CO₃ = 2.25:1) was added dropwise until the pH value reached 7.5. Stirring was continued for another hour. The reaction solution was then transferred to a water bath and reacted at 75°C for 48 hours. After the reaction, the mixture was filtered, washed several times with deionized water and ethanol, and dried in a vacuum drying oven at 60°C for 10-12 hours to obtain Li₁Al₂-LDHs.
[0101] (2) 340 mg Li1Al2-LDHs was added to 40 mL of deionized water and stirred vigorously for 0.5 hours. Then, five metal precursor solutions were added: copper nitrate hexahydrate (1 mL, containing 2.91 mg copper nitrate hexahydrate), nickel nitrate hexahydrate (1 mL, containing 2.91 mg nickel nitrate hexahydrate), ruthenium trichloride trihydrate (1 mL, containing 2.07 mg ruthenium trichloride trihydrate), rhodium trichloride trihydrate (1 mL, containing 2.63 mg rhodium trichloride trihydrate), and sodium chloropalladium (1 mL, containing 2.94 mg sodium chloropalladium). After stirring at room temperature for 1 hour, the solution was evaporated at 80 °C for 10-12 hours until all deionized water was removed. The solution was then transferred to a mortar and ground. The resulting sample was calcined at 400 °C for 4 hours (heating rate 5 °C / min) under a 5% H2 / 95% Ar atmosphere. -1 A high-entropy alloy-like hydrotalcite oxide composite material, denoted as Li1Al2-LDOs / CuNiRuRhPd-HEAs, was obtained. Its high-entropy alloy configuration entropy value is 1.53R, which proves its high-entropy characteristics.
[0102] Methane dry reforming performance test:
[0103] The DRM reaction was carried out in a continuous flow fixed-bed reactor (Beijing Pofilai Technology Co., Ltd.). In the test, 2 mg of Li1Al2-LDOs / CuNiRuRhPd-HEAs prepared in Comparative Example 1 was uniformly dispersed on glass fiber filter paper with a diameter of 3 cm. After the sample was placed in the sealed reactor, the reaction gas (10% CH4 / 10% CO2 / 80% Ar) was introduced at a rate of 10 mL / min. -1 The feed gas was introduced into the reactor at a flow rate of [missing information]. A 300W xenon lamp (PLS-SXE300, Perfect Light) was used as the light source to drive the DRM reaction. After the feed gas reached equilibrium adsorption, the gaseous products were detected by a gas chromatograph (GC97902Ⅱ, Fuli), equipped with two flame ionization detectors (FID) and one thermal conductivity detector (TCD) to evaluate the products.
[0104] The results showed that the yield of H2 / CO was (10.82 / 17.23 mol) -1 g metal -1 h -1 The selectivity was 0.63.
[0105] Comparative Example 2
[0106] (1) First, mix TiCl4 (0.555 mL), CaCl2 (1.665 g), and AlCl3·6H2O (7.245 g) in a flask. 4+ Ca 2+ Al3+ The molar ratio of the substances was 1:3:6. After mixing, the mixture was stirred for 1 hour. Then, while stirring, a mixed solution of KOH and Na₂CO₃ (KOH:Na₂CO₃ = 2.25:1) was added dropwise until the pH reached 7.5. Stirring continued for another hour. The reaction solution was then transferred to a water bath and reacted at 75°C for 48 hours. After the reaction, the mixture was filtered, washed several times with deionized water and ethanol, and dried in a vacuum drying oven at 60°C for 10-12 hours to obtain Ti₁Ca₃Al₆-LDHs.
[0107] (2) 340 mg Ti1Ca3Al6-LDHs was added to 40 mL of deionized water and stirred vigorously for 0.5 hours. Then, five metal precursor solutions were added: copper nitrate hexahydrate (1 mL, containing 2.91 mg copper nitrate hexahydrate), nickel nitrate hexahydrate (1 mL, containing 2.91 mg nickel nitrate hexahydrate), ruthenium trichloride trihydrate (1 mL, containing 2.07 mg ruthenium trichloride trihydrate), rhodium trichloride trihydrate (1 mL, containing 2.63 mg rhodium trichloride trihydrate), and sodium chloropalladium (1 mL, containing 2.94 mg sodium chloropalladium). After stirring at room temperature for 1 hour, the solution was evaporated at 80 °C for 10-12 hours until all deionized water was removed. The solution was then transferred to a mortar and ground. The resulting sample was calcined at 300 °C for 4 hours (heating rate 5 °C / min) under a 5% H2 / 95% Ar atmosphere. -1 A high-entropy alloy-like hydrotalcite oxide composite material, denoted as Ti1Ca3Al6-LDOs / CuNiRuRhPd-HEAs, was obtained. Its high-entropy alloy configuration entropy value is 1.54R, which proves its high-entropy characteristics.
[0108] Methane dry reforming performance test:
[0109] The DRM reaction was carried out in a continuous flow fixed-bed reactor (Beijing Pofilai Technology Co., Ltd.). In the test, 2 mg of the Ti1Ca3Al6-LDOs / CuNiRuRhPd-HEAs prepared in Comparative Example 2 was uniformly dispersed on glass fiber filter paper with a diameter of 3 cm. After the sample was placed in the sealed reactor, the reaction gas (10% CH4 / 10% CO2 / 80% Ar) was introduced at a rate of 10 mL / min. -1 The feed gas was introduced into the reactor at a flow rate of [missing information]. A 300W xenon lamp (PLS-SXE300, Perfect Light) was used as the light source to drive the DRM reaction. After the feed gas reached equilibrium adsorption, the gaseous products were detected by a gas chromatograph (GC97902Ⅱ, Fuli), equipped with two flame ionization detectors (FID) and one thermal conductivity detector (TCD) to evaluate the products.
[0110] The results showed that the yields of H2 / CO were (5.42 / 8.83 mol) -1g metal -1 h -1 The selectivity was 0.61.
[0111] Comparative Example 3
[0112] (1) First, mix TiCl4 (0.555 mL), LiCl (0.635 g), and AlCl3·6H2O (7.245 g) in a flask. 4+ Li + Al 3+ The molar ratio of the substances was 1:3:6. After mixing, the mixture was stirred for 1 hour. Then, while stirring, a mixed solution of KOH and Na₂CO₃ (KOH:Na₂CO₃ = 2.25:1) was added dropwise until the pH reached 7.5. Stirring continued for another hour. The reaction solution was then transferred to a water bath and reacted at 75°C for 48 hours. After the reaction, the mixture was filtered, washed several times with deionized water and ethanol, and dried in a vacuum drying oven at 60°C for 10-12 hours to obtain Ti₁Li₃Al₆-LDHs.
[0113] (2) 340 mg Ti1Li3Al6-LDHs were added to 40 mL of deionized water and stirred vigorously for 0.5 hours. A precursor solution of rhodium trichloride trihydrate (1 mL, containing 2.63 mg of rhodium trichloride trihydrate) was then added. After stirring at room temperature for 1 hour, the mixture was evaporated at 80 °C for 10-12 hours until all deionized water was removed. The mixture was then transferred to a mortar and ground. The resulting sample was calcined at 400 °C for 4 hours (heating rate 5 °C / min) under a 5% H2 / 95% Ar atmosphere. -1 A high-entropy alloy-type hydrotalcite oxide composite material was obtained, denoted as Ti1Li3Al6-LDOs / Rh.
[0114] Methane dry reforming performance test:
[0115] The DRM reaction was carried out in a continuous flow fixed-bed reactor (Beijing Pofilai Technology Co., Ltd.). In the test, 2 mg of Ti1Li3Al6-LDOs / Rh prepared in Comparative Example 3 was uniformly dispersed on glass fiber filter paper with a diameter of 3 cm. After the sample was placed in the sealed reactor, the reaction gas (10% CH4 / 10% CO2 / 80% Ar) was introduced at a rate of 10 mL / min. -1 The feed gas was introduced into the reactor at a flow rate of [missing information]. A 300W xenon lamp (PLS-SXE300, Perfect Light) was used as the light source to drive the DRM reaction. After the feed gas reached equilibrium adsorption, the gaseous products were detected by a gas chromatograph (GC97902Ⅱ, Fuli), equipped with two flame ionization detectors (FID) and one thermal conductivity detector (TCD) to evaluate the products.
[0116] The results showed that the yields of H2 / CO were (1.45 / 3.98 mol) -1 g metal -1 h -1 The selectivity was 0.36.
[0117] By comparing Examples 1-7 with Comparative Examples 1-3, it can be seen that the preparation conditions of this invention have high selectivity and good H2 / CO yield in methane dry reforming.
[0118] The above description is only of the preferred embodiment of the present invention and should not be construed as limiting the scope of the claims. The present invention is not limited to the above embodiments, and variations in its specific structure are permitted. All variations made within the scope of the independent claims of the present invention are also within the scope of protection of the present invention.
[0119] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.
Claims
1. A method for preparing a high-entropy alloy-type hydrotalcite oxide composite material, characterized in that, Includes the following steps: TiCl4, LiCl and AlCl3·6H2O were mixed evenly, the pH was adjusted to 7-8, and then reacted at 75-110℃ for 24-48h. After drying, a hydrotalcite-like material containing titanium, lithium and aluminum was obtained; the molar ratio of TiCl4, LiCl and AlCl3·6H2O was (1-2):3:(2-6). A layered double hydroxide (LDH) material containing titanium-lithium-aluminum was added to deionized water and stirred until homogeneous. Then, a solution containing a metal precursor was added and stirred until homogeneous again. After removing the deionized water, the mixture was calcined under a protective atmosphere to obtain a high-entropy alloy LDH oxide composite material. The ratio of the LDH material containing titanium-lithium-aluminum to deionized water was 230-340 mg: 40 mL; the ratio of the LDH material containing titanium-lithium-aluminum to the metal precursor solution was 230-340 mg: 5 mL. The protective atmosphere comprises, by volume percentage, 5% H2 and 95% Ar; The calcination temperature is 300-500℃, and the time is 2-4 hours; The metal precursor solution was a mixture of 10 mmol / L copper nitrate hexahydrate solution, 10 mmol / L nickel nitrate hexahydrate solution, 10 mmol / L ruthenium trichloride trihydrate solution, 10 mmol / L rhodium trichloride trihydrate solution and 10 mmol / L sodium chloropalladium solution in a volume ratio of 1:1:1:1:
1. or The metal precursor solution was a mixture of 10 mmol / L cobalt nitrate hexahydrate solution, 10 mmol / L nickel nitrate hexahydrate solution, 10 mmol / L ruthenium trichloride trihydrate solution, 10 mmol / L rhodium trichloride trihydrate solution and 10 mmol / L sodium chloropalladium solution in a volume ratio of 1:1:1:1:
1. or The metal precursor solution was a mixture of 10 mmol / L chloroauric acid solution, 10 mmol / L nickel nitrate hexahydrate solution, 10 mmol / L ruthenium trichloride trihydrate solution, 10 mmol / L rhodium trichloride trihydrate solution and 10 mmol / L sodium chloropalladate solution in a volume ratio of 1:1:1:1:1:
1.
2. The preparation method of the high-entropy alloy-type hydrotalcite oxide composite material according to claim 1, characterized in that, The pH was adjusted to 7-8 using a mixed solution of KOH and Na2CO3 with a molar ratio of 2.25:
1.
3. The preparation method of the high-entropy alloy-type hydrotalcite oxide composite material according to claim 1, characterized in that, At 5-10℃ min -1 The heating rate is increased to 300-500℃.
4. A high-entropy alloy-type hydrotalcite oxide composite material prepared according to the method described in claims 1-3.
5. The application of the high-entropy alloy-type hydrotalcite oxide composite material as described in claim 4 in photocatalytic methane dry reforming.