Carbon dioxide selective hydrogenation catalyst, its preparation method and application

By utilizing the Pt NCs@UiO-66(SO₃H)₂ catalyst and the active interface structure formed by zirconium nodes and Pt clusters, the problems of harsh reaction conditions and low activity of copper-based catalysts in the process of carbon dioxide hydrogenation to methanol were solved, and a high selectivity and stable catalytic effect at low temperature was achieved.

CN118616100BActive Publication Date: 2026-11-20THE NAT CENT FOR NANOSCI & TECH NCNST OF CHINA
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410685766.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-30
Publication Date
2026-11-20
Estimated Expiration
2044-05-30

AI Technical Summary

Technical Problem

Existing copper-based catalysts exhibit harsh reaction conditions and low activity in the process of producing methanol from carbon dioxide. Furthermore, the deactivation and dynamic changes of active sites are difficult to define, resulting in poor catalytic performance at low temperatures.

Method used

The catalyst is Pt NCs@UiO-66(SO₃H)₂, which consists of a metal-organic framework UiO-66(SO₃H)₂ and Pt clusters supported in its channels. The active interface structure is formed by the zirconium nodes exposed at the defects in the metal-organic framework and the Pt clusters. High selectivity and long-term stability are achieved by precisely controlling the active interface.

Benefits of technology

High selectivity and long-term stability of carbon dioxide hydrogenation to methanol were achieved under low-temperature conditions, overcoming the problem of insufficient catalytic performance of traditional catalysts at low temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118616100B_ABST
    Figure CN118616100B_ABST
Patent Text Reader

Abstract

The application provides a carbon dioxide selective hydrogenation catalyst and a preparation method and application thereof, and the catalyst is Pt NCs@UiO-66(SO3H)2; the catalyst Pt NCs@UiO-66(SO3H)2 comprises UiO-66(SO3H)2 and Pt clusters distributed in the pores of the UiO-66(SO3H)2. The catalyst provided by the application utilizes the zirconium nodes exposed in the metal organic framework defects and the functionalized ligands to jointly stabilize the small-size Pt clusters, so that the exposed zirconium nodes and the Pt clusters form a precise, rich and controllable active interface structure; compared with the traditional supported catalyst, the catalyst exhibits more excellent performance in the reaction of CO2 hydrogenation to methanol, and can realize the CO2 hydrogenation synthesis of methanol with high selectivity and long-time stability under low-temperature conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of catalytic hydrogenation technology, and relates to a catalyst for selective hydrogenation of carbon dioxide, its preparation method and application. Background Technology

[0002] Compared to separation, adsorption, and storage methods, utilizing gas-solid phase catalytic hydrogenation of carbon dioxide to obtain a series of high-value-added downstream products is of greater significance for reducing CO2 concentration and realizing the recycling of carbon resources. Among the products, methanol, as an important synthetic intermediate, solvent, and fuel resource, is the cornerstone of the "methanol economy." Currently, the production of methanol from CO2 mainly uses copper-based catalysts, especially Cu / ZnO / Al2O3. However, copper-based catalysts suffer from harsh reaction conditions, low reactivity, and difficulty in defining deactivation and dynamic changes in active sites.

[0003] Various measures have been studied to improve the activity of existing catalysts. For example, patent CN111167518A modifies the support by selecting the metal-organic framework UiO-66, composed of Zr6O8 clusters and terephthalic acid, as a novel support. Cu and Zn particles are loaded using a co-precipitation method. Through the synergistic effect between the UiO-66 metal nodes and CuZn sites, nearly 50% methanol selectivity is achieved under reaction conditions of 240℃ and 3MPa. Similarly, patent CN114029063A improves the catalytic activity of CuZnZr catalysts for methanol synthesis by adding metal promoters and carbon materials. Using Al as the metal promoter and silicon carbide as the added carbon material, methanol selectivity can be increased to approximately 80% under reaction conditions of 240℃ and 3MPa. Finally, patent CN114920623A significantly improves the hydrophobic properties of the Cu / ZnO / Al2O3 catalyst by surface silanization, thereby enhancing methanol selectivity.

[0004] As mentioned above, although various types of catalysts and modification methods have been disclosed in the prior art, the production of methanol from CO2 via hydrogenation remains limited by harsh reaction temperatures, low reaction selectivity, and low stability. Therefore, there is an urgent need to develop a catalyst for the selective hydrogenation of carbon dioxide and its preparation method to achieve highly selective and stable production of methanol from CO2 via hydrogenation under mild conditions. Summary of the Invention

[0005] To address the shortcomings of existing technologies, the present invention aims to provide a catalyst for the selective hydrogenation of carbon dioxide, its preparation method, and its application. The catalyst is Pt NCs@UiO-66(SO3H)2, which consists of a metal-organic framework material UiO-66(SO3H)2 and Pt clusters supported in its pores. The catalyst has an active interface structure formed by zirconium nodes exposed at defects in the metal-organic framework and Pt clusters. Compared with traditional supported catalysts, the catalyst exhibits superior performance in the selective hydrogenation of carbon dioxide, overcoming the problem that traditional catalysts are difficult to catalyze the hydrogenation of carbon dioxide under low-temperature conditions, and achieving high selectivity and long-term stability in the catalytic hydrogenation of carbon dioxide to methanol under low-temperature conditions.

[0006] To achieve this objective, the present invention adopts the following technical solution:

[0007] In a first aspect, the present invention provides a catalyst for selective hydrogenation of carbon dioxide, wherein the catalyst is PtNCs@UiO-66(SO3H)2;

[0008] The Pt NCs@UiO-66(SO3H)2 comprises a metal-organic framework UiO-66(SO3H)2 and Pt clusters distributed in the pores of the metal-organic framework UiO-66(SO3H)2.

[0009] The catalyst Pt NCs@UiO-66(SO3H)2 provided by this invention is obtained by solvothermal synthesis of a metal-organic framework (UiO-66(SH)2) composed of an organic mixed ligand consisting of terephthalic acid and 2,5-dimercaptoterephthalic acid and zirconium tetrachloride, followed by ligand oxidation to obtain UiO-66(SO3H)2, and then loading Pt clusters in its channels. In the catalyst, the zirconium nodes exposed at the defects in the metal-organic framework and the functionalized ligands jointly stabilize the small-sized Pt clusters, thereby forming an active interface structure with the exposed zirconium nodes and Pt clusters. This active interface structure is precise, abundant and easily tunable. The catalyst exhibits superior performance in the selective hydrogenation reaction of carbon dioxide compared to traditional supported catalysts, and can achieve high selectivity and long-term stability in the catalytic hydrogenation of carbon dioxide to methanol under low-temperature conditions.

[0010] Preferably, the metal-organic framework UiO-66(SO3H)2 contains 10-50% molar content of sulfonated ligands and 50-90% molar content of non-sulfonated ligands.

[0011] The UiO-66(SO3H)2 of the present invention contains 10 to 50% molar content of sulfonated ligand, for example, 10%, 15%, 20%, 25%, 30%, 35%, 45%, 45%, or 50%, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0012] The non-sulfonated ligand in the UiO-66(SO3H)2 of the present invention has a molar content of 50 to 90%, for example, it can be 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85% or 90%, but is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0013] Preferably, the Pt clusters are distributed in the channels of the metal-organic framework UiO-66(SO3H)2 and are fixed by zirconium nodes exposed at defects in the metal-organic framework UiO-66(SO3H)2 and sulfonic acid groups on the ligands.

[0014] Preferably, the particle size distribution of the Pt clusters is 0.6–2 nm, for example, it can be 0.6–0.8 nm, 0.6–1 nm, 0.6–1.5 nm, 0.6–2 nm, 0.7–0.8 nm, 0.7–1 nm, 0.7–1.5 nm, 0.7–2 nm, 1.2–1.6 nm, 1.2–2 nm, 1.5–1.8 nm, or 1.8–2 nm, but it is not limited to the listed numerical ranges. Other unlisted numerical ranges within this range are also applicable.

[0015] In a second aspect, the present invention provides a method for preparing the catalyst described in the first aspect, the method comprising:

[0016] A Pt source, UiO-66(SO3H)2 and a solvent were mixed and then thermally reduced in a protective atmosphere containing reducing gases to obtain a Pt NCs@UiO-66(SO3H)2 catalyst.

[0017] The protective atmosphere described in this invention includes an inert atmosphere and / or a nitrogen atmosphere, wherein the inert atmosphere includes any one of a helium atmosphere, a neon atmosphere, an argon atmosphere, or a krypton atmosphere.

[0018] The catalyst preparation method provided by this invention can precisely control the active interface structure formed by zirconium metal nodes exposed at defects in the metal-organic framework UiO-66(SO3H)2 and Pt clusters.

[0019] Preferably, the Pt source includes any one or a combination of at least two of potassium tetrachloroplatinate, chloroplatinic acid, or platinum nitrate. Typical but non-limiting combinations include a combination of potassium tetrachloroplatinate and chloroplatinic acid, a combination of chloroplatinic acid and platinum nitrate, or a combination of potassium tetrachloroplatinate, chloroplatinic acid, and platinum nitrate.

[0020] Preferably, the solvent in the mixture is water.

[0021] Preferably, the mixing includes: mixing a Pt source with a portion of the solvent to obtain a first mixture; mixing UiO-66(SO3H)2 with the remaining solvent to obtain a second mixture; adding the obtained first mixture dropwise to the obtained second mixture, and then stirring.

[0022] Preferably, the mass ratio of the Pt source to the metal-organic framework UiO-66(SO3H)2 is (0.01 to 0.1):1, for example, it can be 0.01:1, 0.02:1, 0.03:1, 0.04:1, 0.05:1, 0.06:1, 0.07:1, 0.08:1, 0.09:1 or 0.1:1, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0023] Preferably, the solid-liquid ratio of the Pt source to the partial solvent is (2.1 to 9.6):1, for example, it can be 2.1:1, 3.2:1, 4.2:1, 5.3:1, 6.3:1, 7.4:1, 8.4:1 or 9.6:1, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable. The unit of the solid-liquid ratio is mg / mL.

[0024] Preferably, the solid-liquid ratio of UiO-66(SO3H)2 to the remaining solvent is (15-25):1, for example, it can be 15:1, 16:1, 17:1, 18:1, 19:1, 20:1, 21:1, 22:1, 23:1, 24:1 or 25:1, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable. The unit of the solid-liquid ratio is mg / mL.

[0025] Preferably, the stirring time is 10 to 15 hours, for example, 10 hours, 10.5 hours, 11 hours, 11.5 hours, 12 hours, 12.5 hours, 13 hours, 13.5 hours, 14 hours, 14.5 hours or 15 hours, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0026] Preferably, after the stirring process is completed, the mixture is centrifuged and washed in sequence, and then placed in a vacuum oven to dry.

[0027] Preferably, the volume concentration of the reducing gas in the protective atmosphere is 5% to 15%, for example, it can be 5%, 6%, 7%, 8%, 9%, 10%, 11%, 12%, 13%, 14% or 15%, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0028] Preferably, the reducing gas is hydrogen.

[0029] Preferably, the thermal reduction includes sequential heating and holding, wherein the heating rate is 1-5℃ / min, the final temperature is 180-220℃, and the holding time is 1.5-2.5h.

[0030] The heating rate described in this invention is 1 to 5 °C / min, for example, it can be 1 °C / min, 2 °C / min, 3 °C / min, 4 °C / min or 5 °C / min, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0031] The endpoint temperature for heating described in this invention is 180 to 220°C, for example, it can be 180°C, 185°C, 190°C, 195°C, 200°C, 205°C, 210°C, 215°C or 220°C, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0032] The heat preservation time described in this invention is 1.5 to 2.5 hours, for example, it can be 1.5 hours, 1.6 hours, 1.7 hours, 1.8 hours, 1.9 hours, 2.0 hours or 2.5 hours, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0033] Preferably, the method for preparing the metal-organic framework UiO-66(SO3H)2 includes:

[0034] The metal precursor, organic mixed ligand and organic solvent are mixed and then thermally synthesized to obtain UiO-66(SH)2. Then, the ligand is oxidized to obtain UiO-66(SO3H)2.

[0035] Preferably, the metal precursor is zirconium tetrachloride.

[0036] Preferably, the organic mixed ligand is terephthalic acid and 2,5-dimercaptoterephthalic acid.

[0037] Preferably, the organic solvent is N,N-dimethylformamide.

[0038] Preferably, the mixture further includes glacial acetic acid and water.

[0039] Preferably, the volume of the organic solvent in the mixture is fixed at 45-55 mL, for example, it can be 45 mL, 47 mL, 49 mL, 51 mL, 53 mL or 55 mL, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0040] Preferably, the molar ratio of zirconium tetrachloride to terephthalic acid in the mixture is 1:(0.6 to 0.9), for example, it can be 1:0.6, 1:0.65, 1:0.7, 1:0.75, 1:0.8, 1:0.85 or 1:0.9, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0041] Preferably, the molar ratio of terephthalic acid to 2,5-dimercaptoterephthalic acid in the mixture is (1-9):1, for example, it can be 1:1, 11:9, 1.5:1, 13:7, 7:3, 3:1, 4:1, 17:3 or 9:1, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0042] Preferably, the molar ratio of zirconium tetrachloride to glacial acetic acid in the mixture is 1:(25-175), for example, it can be 1:25, 1:50, 1:75, 1:100, 1:125 or 1:175, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0043] Preferably, the molar ratio of zirconium tetrachloride to water in the mixture is 1:(2-4); for example, it can be 1:2, 1:2.5, 1:3, 1:3.5 or 1:4, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0044] Preferably, the temperature for thermal synthesis is 110–130°C, and the time is 20–28 hours.

[0045] The thermal synthesis temperature described in this invention is 110 to 130°C, for example, it can be 110°C, 115°C, 120°C, 125°C or 130°C, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0046] The thermal synthesis time described in this invention is 20 to 28 hours, for example, it can be 20 hours, 21 hours, 22 hours, 23 hours, 24 hours, 25 hours, 26 hours, 27 hours or 28 hours, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0047] Preferably, after the thermal synthesis is completed, the product is centrifuged and washed sequentially, and then placed in a vacuum oven to dry, thus obtaining a solid.

[0048] Preferably, the cleaning process includes cleaning three times each with N,N-dimethylformamide and acetone.

[0049] Preferably, the ligand oxidation is performed by oxidizing the thiol group on the 2,5-dimercaptophthalic acid ligand in the thermally synthesized solid UiO-66(SH)2 to form a sulfonic acid group.

[0050] Preferably, the oxidation includes: dispersing the solid UiO-66(SH)2 obtained after thermal synthesis in a 15-45% hydrogen peroxide aqueous solution and stirring the reaction.

[0051] In this invention, the volume concentration of hydrogen peroxide is 15% to 45%, for example, it can be 15%, 20%, 25%, 30%, 35%, 40% or 45%, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0052] Preferably, the solid-liquid ratio of the thermally synthesized solid UiO-66(SH)2 to the hydrogen peroxide solution is (8-12):1, for example, it can be 8:1, 8.5:1, 9:1, 9.5:1, 10:1, 10.5:1, 11:1, 11.5:1 or 12:1, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable. The unit of the solid-liquid ratio is mg / mL.

[0053] Preferably, the stirring reaction time is 20 to 28 hours, for example, 20 hours, 21 hours, 22 hours, 23 hours, 24 hours, 25 hours, 26 hours, 27 hours or 28 hours, but it is not limited to the listed values. Other unlisted values ​​within this range are also applicable.

[0054] Preferably, all stirring reactions are carried out under light-protected conditions.

[0055] As a preferred embodiment of the preparation method of the present invention, the preparation method includes:

[0056] (1) Zirconium tetrachloride, glacial acetic acid, water, terephthalic acid, 2,5-dimercaptoterephthalic acid and 45-55 mL of N,N-dimethylformamide were mixed and then thermally synthesized at 110-130 °C for 20-28 h. After centrifugation, washing and drying, solid UiO-66(SH)2 was obtained. The obtained solid UiO-66(SH)2 was dispersed in a 15-45% hydrogen peroxide solution. The solid-liquid ratio of the solid UiO-66(SH)2 to the hydrogen peroxide solution was (8-12):1, and the unit of the solid-liquid ratio was mg / mL. The reaction was carried out in the dark for 20-28 h with stirring to obtain UiO-66(SO3H)2.

[0057] The molar ratio of zirconium tetrachloride to terephthalic acid in the mixture is 1:(0.6-0.9), the molar ratio of terephthalic acid to 2,5-dimercaptoterephthalic acid is (1-9):1, the molar ratio of zirconium tetrachloride to glacial acetic acid is 1:(25-175), and the molar ratio of zirconium tetrachloride to water is 1:(2-4).

[0058] (2) Mix Pt source with part of solvent water to obtain a first mixture; mix UiO-66(SO3H)2 with the remaining solvent water to obtain a second mixture; add the obtained first mixture to the obtained second mixture dropwise, and then stir for 10-15 hours. After centrifugation, washing and drying, a solid powder is obtained.

[0059] The mass ratio of the Pt source to UiO-66(SO3H)2 is (0.01~0.1):1, the solid-liquid ratio of the Pt source to the partial solvent water is (2.1~9.6):1, and the solid-liquid ratio of UiO-66(SO3H)2 to the remaining solvent water is (15~25):1. The unit of the solid-liquid ratio is mg / mL.

[0060] (3) The solid powder obtained in step (2) is heated to 180-220°C at a rate of 1-5°C / min in a protective atmosphere of 5-15% hydrogen volume concentration and then kept at the temperature for 1.5-2.5h to obtain Pt NCs@UiO-66(SO3H)2 catalyst.

[0061] Thirdly, the present invention provides an application of the catalyst described in the first aspect, wherein the catalyst is used to catalyze the hydrogenation reaction of carbon dioxide.

[0062] Compared with the prior art, the present invention has the following beneficial effects:

[0063] (1) The catalyst Pt NCs@UiO-66(SO3H)2 provided by the present invention is obtained by ligand oxidation of a metal-organic framework (UiO-66(SH)2) synthesized from zirconium tetrachloride with an organic mixed ligand system composed of thiol-functionalized ligands and non-functionalized ligands to obtain UiO-66(SO3H)2, and then loading Pt clusters in its channels; the catalyst utilizes the zirconium nodes exposed at the defects in the metal-organic framework and the functionalized ligands to stabilize the small-sized Pt clusters, thereby forming an active interface structure with the exposed zirconium nodes and Pt clusters. This active interface structure is precise, abundant and easy to control.

[0064] (2) The catalyst provided by the present invention exhibits superior performance in the selective hydrogenation reaction of carbon dioxide compared with traditional supported catalysts. It can overcome the problem that traditional catalysts are difficult to catalyze the hydrogenation of carbon dioxide under low temperature conditions, and realize the synthesis of methanol by catalytic hydrogenation of carbon dioxide with high selectivity and long-term stability under low temperature conditions. Attached Figure Description

[0065] Figure 1 The image shows the SEM image of UiO-66(SH)2 obtained in Example 1.

[0066] Figure 2 The image shows the SEM image of UiO-66(SO3H)2 obtained in Example 1.

[0067] Figure 3 This is a low-magnification, aberration-corrected, high-angle annular dark-field scanning transmission electron microscope image of Pt NCs@UiO-66(SO3H)2 provided in Example 1.

[0068] Figure 4 This is a high-magnification, aberration-corrected, high-angle annular dark-field scanning transmission electron microscope image of Pt NCs@UiO-66(SO3H)2 provided in Example 1.

[0069] Figure 5 This is a high-magnification, aberration-corrected, high-angle annular dark-field scanning transmission electron microscope image of Pt NCs@UiO-66(SO3H)2 provided in Example 1.

[0070] Figure 6 This is a particle size distribution diagram of Pt clusters in Pt NCs@UiO-66(SO3H)2 provided in Example 1.

[0071] Figure 7 The image shows a high-angle annular dark-field scanning transmission electron microscope image and its elemental distribution diagram of Pt NCs@UiO-66(SO3H)2 provided in Example 1.

[0072] Figure 8 The image shows the XRD pattern of UiO-66(SH)2 obtained in Example 1.

[0073] Figure 9 The image shows the XRD pattern of UiO-66(SO3H)2 obtained in Example 1.

[0074] Figure 10 The image shows the XRD pattern of Pt NCs@UiO-66(SO3H)2 provided in Example 1.

[0075] Figure 11 This is a stability test graph showing the change in methanol space-time yield of Pt NCs@UiO-66(SO3H)2 provided in Example 1 as a function of reaction time.

[0076] Figure 12 This is a high-magnification, aberration-corrected, high-angle annular dark-field scanning transmission electron microscope image of Pt NCs@UiO-66(SO3H)2 provided in Example 1 after undergoing a CO2 hydrogenation reaction.

[0077] Figure 13 The particle size distribution of Pt clusters in Pt NCs@UiO-66(SO3H)2 provided in Example 1 after CO2 hydrogenation reaction is shown.

[0078] Figure 14 The image shows the XRD pattern of Pt NCs@UiO-66(SO3H)2 provided in Example 1 after CO2 hydrogenation reaction. Detailed Implementation

[0079] The technical solution of the present invention will be further illustrated below through specific embodiments. Those skilled in the art should understand that the embodiments described are merely illustrative of the present invention and should not be construed as limiting the invention in any way.

[0080] Example 1

[0081] This embodiment provides a selective hydrogenation catalyst for carbon dioxide based on a metal-organic framework material. The catalyst is Pt NCs@UiO-66(SO3H)2, which includes UiO-66(SO3H)2 and Pt clusters distributed in the pores of UiO-66(SO3H)2.

[0082] The UiO-66(SO3H)2 contains 20% molar content of sulfonated ligands and 80% of non-sulfonated ligands;

[0083] The Pt clusters have a particle size distribution of 0.6-2 nm and an average particle size of 1.49 nm.

[0084] The method for preparing the catalyst includes:

[0085] (1) Take 431 mg zirconium tetrachloride, 10.571 mL glacial acetic acid and 0.1 mL water and dissolve them in 25 mL N,N-dimethylformamide. Separately, take 245.65 mg terephthalic acid and 85.09 mg 2,5-dimercaptoterephthalic acid and dissolve them in 25 mL N,N-dimethylformamide. Mix the two solutions evenly and heat them in a constant temperature oven at 120 °C for 24 h. Centrifuge, wash three times with N,N-dimethylformamide and acetone respectively, and dry in a vacuum oven to obtain UiO-66(SH)2.

[0086] Take 250 mg of the obtained UiO-66(SH)2 and disperse it in 25 mL of 30% hydrogen peroxide solution. Stir and react for 24 h in the dark. Centrifuge and wash with water four times to obtain UiO-66(SO3H)2, which is then dispersed in 12 mL of water.

[0087] (2) Dissolve 10.6 mg of potassium tetrachloroplatinate in 5 mL of water to obtain the first mixture; use 12 mL of aqueous solution containing UiO-66(SO3H)2 dispersed in (1) as the second mixture; add the obtained first mixture to the obtained second mixture dropwise, stir for 14 h, centrifuge, wash with water 1-2 times, and dry in a vacuum oven to obtain solid powder.

[0088] (3) The solid powder obtained in step (2) is heated to 200°C at a rate of 1°C / min in an argon atmosphere with a hydrogen volume concentration of 10% and then kept at the temperature for 2 hours to obtain the solid powder catalyst Pt NCs@UiO-66(SO3H)2.

[0089] Example 2

[0090] This embodiment provides a selective hydrogenation catalyst for carbon dioxide based on a metal-organic framework material. The difference between this catalyst and Example 1 is that the UiO-66(SO3H)2 contains 10% sulfonated ligands and 90% non-sulfonated ligands. Specifically, the amount of terephthalic acid is 276.61 mg and the amount of 2,5-dimercaptoterephthalic acid is 42.60 mg. All other substances, amounts, and steps are the same as in Example 1.

[0091] Example 3

[0092] This embodiment provides a selective hydrogenation catalyst for carbon dioxide based on a metal-organic framework material. The difference between this catalyst and Example 1 is that the UiO-66(SO3H)2 contains 40% sulfonated ligands and 60% non-sulfonated ligands. Specifically, the amount of terephthalic acid is 184.40 mg and the amount of 2,5-dimercaptoterephthalic acid is 170.39 mg. All other substances, amounts, and steps are the same as in Example 1.

[0093] Example 4

[0094] This embodiment provides a selective hydrogenation catalyst for carbon dioxide based on a metal-organic framework material. The difference between this catalyst and Example 1 is the change in the amount of Pt source. The mass ratio of Pt source to UiO-66(SO3H)2 is increased to 0.09:1, specifically by increasing the amount of potassium tetrachloroplatinate to 48 mg. All other substances, amounts, and steps are the same as in Example 1.

[0095] Example 5

[0096] This embodiment provides a selective hydrogenation catalyst for carbon dioxide based on a metal-organic framework material. The difference between this catalyst and Example 1 is the change in the amount of glacial acetic acid used. The molar ratio of zirconium tetrachloride to glacial acetic acid is changed to 1:50, specifically, the amount of glacial acetic acid used is reduced to 5.286 mL. All other substances, amounts, and steps are the same as in Example 1.

[0097] Example 6

[0098] This embodiment provides a selective hydrogenation catalyst for carbon dioxide based on a metal-organic framework material. The difference between this catalyst and Example 1 is the change in the amount of glacial acetic acid used. The molar ratio of zirconium tetrachloride to glacial acetic acid is changed to 1:150, specifically, the amount of glacial acetic acid is increased to 15.857 mL. All other substances, amounts, and steps are the same as in Example 1.

[0099] Example 7

[0100] This embodiment provides a selective hydrogenation catalyst for carbon dioxide based on a metal-organic framework material. The difference between this catalyst and Example 1 is that the UiO-66(SO3H)2 contains 5% sulfonated ligands and 95% non-sulfonated ligands. Specifically, the amount of terephthalic acid is 291.98 mg and the amount of 2,5-dimercaptoterephthalic acid is 21.30 mg. All other substances, amounts, and steps are the same as in Example 1.

[0101] Example 8

[0102] This embodiment provides a selective hydrogenation catalyst for carbon dioxide based on a metal-organic framework material. The difference between this catalyst and Example 1 is that the UiO-66(SO3H)2 contains 60% sulfonated ligands and 40% non-sulfonated ligands. Specifically, the amount of terephthalic acid is 122.94 mg and the amount of 2,5-dimercaptoterephthalic acid is 255.60 mg. All other substances, amounts, and steps are the same as in Example 1.

[0103] Example 9

[0104] This embodiment provides a selective hydrogenation catalyst for carbon dioxide based on a metal-organic framework material. The difference between this catalyst and Example 1 is the change in the amount of Pt source. The mass ratio of Pt source to UiO-66(SO3H)2 is reduced to 0.005:1, specifically by reducing the amount of potassium tetrachloroplatinate by 2.65 mg. All other substances, amounts, and steps are the same as in Example 1.

[0105] Example 10

[0106] This embodiment provides a selective hydrogenation catalyst for carbon dioxide based on a metal-organic framework material. The difference between this catalyst and Example 1 is the change in the amount of Pt source. The mass ratio of Pt source to UiO-66(SO3H)2 is increased to 0.12:1, specifically by increasing the amount of potassium tetrachloroplatinate to 63.6 mg. All other substances, amounts, and steps are the same as in Example 1.

[0107] Example 11

[0108] This embodiment provides a selective hydrogenation catalyst for carbon dioxide based on a metal-organic framework material. The difference between this catalyst and Example 1 is the change in the amount of glacial acetic acid used. The molar ratio of zirconium tetrachloride to glacial acetic acid is changed to 1:15, specifically, the amount of glacial acetic acid used is reduced to 1.586 mL. All other substances, amounts, and steps are the same as in Example 1.

[0109] Example 12

[0110] This embodiment provides a selective hydrogenation catalyst for carbon dioxide based on a metal-organic framework material. The difference between this catalyst and Example 1 is the change in the amount of glacial acetic acid used. The molar ratio of zirconium tetrachloride to glacial acetic acid is changed to 1:200, specifically, the amount of glacial acetic acid is increased to 21.142 mL. All other substances, amounts, and steps are the same as in Example 1.

[0111] Comparative Example 1

[0112] This comparative example provides a selective hydrogenation catalyst for carbon dioxide based on a metal-organic framework material. The catalyst is Pt NPs / UiO-66, which includes UiO-66 and Pt nanoparticles supported on the UiO-66. The UiO-66 is a metal-organic framework material known in the art, which is solvothermal synthesized from zirconium tetrachloride and terephthalic acid.

[0113] The Pt nanoparticles have a particle size distribution of 3–8 nm and an average particle size of 5.41 nm.

[0114] The method for preparing the catalyst includes:

[0115] (1) Take 431 mg zirconium tetrachloride, 5.286 mL glacial acetic acid and 0.1 mL water and dissolve them in 25 mL N,N-dimethylformamide. Take another 307.34 mg terephthalic acid and dissolve it in 25 mL N,N-dimethylformamide. Mix the two solutions evenly and heat them in a constant temperature oven at 120 °C for 24 h. Centrifuge, wash three times with N,N-dimethylformamide and acetone respectively, and dry in a vacuum oven to obtain UiO-66.

[0116] (2) Dissolve 3.71 mg of potassium tetrachloroplatinate in 5 mL of water to obtain the first mixture; disperse UiO-66 in 12 mL of water as the second mixture; add the first mixture to the second mixture, stir for 14 h, centrifuge, wash with water 1-2 times, and dry in a vacuum oven to obtain solid powder.

[0117] (3) The solid powder obtained in step (2) is heated to 200°C at a rate of 1°C / min in an argon atmosphere with a hydrogen volume concentration of 10% and then kept at the temperature for 2 hours to obtain the solid powder catalyst Pt NPs / UiO-66.

[0118] Comparative Example 2

[0119] This comparative example provides a catalyst for selective hydrogenation of carbon dioxide, wherein the catalyst is Pt / ZrO2, and the Pt / ZrO2 comprises ZrO2 and Pt nanoparticles supported on ZrO2;

[0120] The Pt nanoparticles have a particle size distribution of 2-8 nm and an average particle size of 4.72 nm.

[0121] The method for preparing the catalyst includes:

[0122] (1) Dissolve 12.77 mg of potassium tetrachloroplatinate in 2 mL of water to obtain the first mixture; disperse 1 g of ZrO2 purchased from Inokai Technology Co., Ltd. in 5 mL of water as the second mixture; add the first mixture to the second mixture, stir for 24 h, and remove water by heating in an oil bath at 80 °C to obtain solid powder.

[0123] (2) The solid powder obtained in step (1) is heated to 200°C at a rate of 1°C / min in an argon atmosphere with a hydrogen volume concentration of 10% and then kept at the temperature for 2 hours to obtain the solid powder catalyst Pt / ZrO2.

[0124] Comparative Example 3

[0125] This comparative example provides a catalyst for the selective hydrogenation of carbon dioxide, wherein the catalyst is Pt / Al2O3, and the Pt / Al2O3 comprises Al2O3 and Pt nanoparticles supported on Al2O3;

[0126] The Pt nanoparticles have a particle size distribution of 2-7.5 nm and an average particle size of 4.19 nm.

[0127] The method for preparing the catalyst includes:

[0128] (1) Dissolve 12.77 mg of potassium tetrachloroplatinate in 2 mL of water to obtain the first mixture; disperse 1 g of Al2O3 purchased from Alfaesa in 5 mL of water as the second mixture; add the first mixture to the second mixture, stir for 24 h, and remove water by heating in an oil bath at 80 °C to obtain solid powder.

[0129] (2) The solid powder obtained in step (1) is heated to 200°C at a rate of 1°C / min in an argon atmosphere with a hydrogen volume concentration of 10% and then kept at the temperature for 2 hours to obtain solid powder catalyst Pt / Al2O3.

[0130] Performance testing:

[0131] (1) Scanning Electron Microscopy (SEM): The UiO-66(SH)2 and UiO-66(SO3H)2 obtained in step (1) of the catalyst preparation method described in Example 1 were subjected to SEM using an ultra-high resolution cold field emission scanning electron microscope (Hitachi-SU8220). The SEM images of UiO-66(SH)2 are shown below. Figure 1 As shown, the SEM image of UiO-66(SO3H)2 is obtained as follows. Figure 2 As shown; by Figure 1 and Figure 2 It can be seen that the morphology and size of UiO-66(SO3H)2 obtained after oxidation of UiO-66(SH)2 remain unchanged; the catalysts prepared in Examples 2-6 were also subjected to scanning electron microscopy tests, and the same conclusions as in Example 1 were obtained.

[0132] (2) Transmission Electron Microscopy (TEM) Testing: The size and distribution of Pt clusters in the catalyst PtNCs@UiO-66(SO3H)2 provided in Example 1 were characterized using a field emission transmission electron microscope (Tecnai G2 F20 U-TWIN) and an aberration-corrected transmission electron microscope (FEI Titan Cubed Themis G2 300). The low-magnification aberration-corrected high-angle annular dark-field scanning electron microscope image of the catalyst PtNCs@UiO-66(SO3H)2 is shown below. Figure 3 As shown, the high-magnification, aberration-corrected, high-angle annular dark-field scanning electron microscope image of the obtained catalyst Pt NCs@UiO-66(SO3H)2 is as follows. Figure 4 and 5 As shown, the particle size distribution of Pt clusters in the obtained catalyst Pt NCs@UiO-66(SO3H)2 is as follows: Figure 6 As shown, the high-angle annular dark-field scanning transmission electron microscope (STEM) image and elemental distribution diagram of the obtained catalyst Pt NCs@UiO-66(SO3H)2 are as follows. Figure 7As shown, it can be observed that in the catalyst Pt NCs@UiO-66(SO3H)2 provided in Example 1, the Pt clusters are uniformly distributed in the pores of UiO-66(SO3H)2, with small and uniform size, and no obviously large Pt nanoparticles. The catalysts prepared in Examples 2-6 were also subjected to transmission electron microscopy tests, and the same conclusions as in Example 1 were obtained. Among them, the Pt cluster particle size distribution in the catalyst Pt NCs@UiO-66(SO3H)2 provided in Example 1 is 0.6-2 nm, and the average particle size is 1.49 nm.

[0133] (3) XRD test: X-ray diffractometer (Rigaku D / MAX-TTRIII) was used to test the UiO-66(SH)2 and UiO-66(SO3H)2 obtained in step (1) of the catalyst preparation method described in Example 1, and the Pt NCs@UiO-66(SO3H)2 obtained in step (3). The XRD pattern of UiO-66(SH)2 is shown in the figure. Figure 8 As shown, the XRD pattern of the obtained UiO-66(SO3H)2 is as follows. Figure 9 As shown, the XRD pattern of Pt NCs@UiO-66(SO3H)2 is as follows. Figure 10 As shown; by Figures 8-10 It can be seen that the synthesized UiO-66(SH)2 has a good crystal structure. After subsequent synthesis of UiO-66(SO3H)2 and Pt NCs@UiO-66(SO3H)2, the crystal structure remains unchanged. The catalysts prepared in Examples 2-6 were also subjected to XRD tests, and the same conclusions as in Example 1 were obtained.

[0134] (4) Performance test of selective carbon dioxide hydrogenation: The catalysts provided in Examples 1-6 and Comparative Examples 1-3 were subjected to a catalytic test for selective carbon dioxide hydrogenation. The catalytic test for selective carbon dioxide hydrogenation was as follows: 300 mg of the selective carbon dioxide hydrogenation catalyst was mixed with 1.8 g of 40-60 mesh quartz sand and packed into a stainless steel reaction tube with an inner diameter of 8 mm. The two ends of the packing layer were fixed with quartz wool. Hydrogen and carbon dioxide were introduced as reaction gases, and the mixing ratio was controlled at 3:1. The temperature was raised to 250 °C to activate the catalyst and remove adsorbed pollutants. Subsequently, the temperature was lowered and controlled at 60 °C, while the pressure was controlled at 3 MPa and the gas flow rate was 10 mL / min, i.e., the space velocity was 2000 mL g. cat -1 h -1Catalytic carbon dioxide hydrogenation tests were conducted. Each steady-state catalytic data point was collected using a gas chromatograph (Shimadzu GC-2014C, Japan) equipped with two flame ionization detectors (FID) and one thermal conductivity detector (TCD) after at least one day of stabilization. The space-time yield and selectivity of methanol were calculated based on the peak areas of carbon monoxide, methane, and methanol, combined with the standard curves for each substance. The catalytic results are shown in Table 1.

[0135] Table 1

[0136]

[0137]

[0138] From Table 1, we can obtain:

[0139] The selective hydrogenation catalysts for carbon dioxide provided in Examples 1 to 6 of this invention were used to carry out the catalytic hydrogenation reaction of carbon dioxide. At a low temperature of 60°C, they can exhibit high activity in the selective hydrogenation of carbon dioxide to produce methanol, as shown in Table 1, and have high methanol selectivity.

[0140] A comparison of Examples 1 with Examples 7 and 8 reveals that the proportion of sulfonated ligands in the UiO-66(SO3H)2 of the selective carbon dioxide hydrogenation catalyst provided by this invention affects the catalyst's performance: an appropriate proportion of sulfonated ligands ensures the stable formation of small-sized Pt clusters, allowing the Pt clusters to form abundant active interfaces with the zirconium nodes exposed at the defects in the UiO-66(SO3H)2; an excessively low number of sulfonated ligands reduces the active interface, resulting in a decrease in both methanol yield and selectivity; an excessively high number of sulfonated ligands leads to smaller pores in the UiO-66(SO3H)2, affecting mass transfer and causing a decrease in methanol yield.

[0141] A comparison of the catalytic results of Examples 1 with those of Examples 9 and 10 shows that the loading of Pt clusters in the selective hydrogenation catalyst for carbon dioxide provided by the present invention affects the performance of the catalyst: when the loading of Pt clusters is too low, fewer Pt clusters will be formed, resulting in fewer active sites and a decrease in methanol yield; when the loading of Pt clusters is too high, Pt clusters will agglomerate into large nanoparticles, resulting in an uneven active interface and too many Pt(111) crystal faces, which will reduce methanol selectivity.

[0142] A comparison of Example 1 with Examples 11 and 12 reveals that the amount of glacial acetic acid added in the preparation method of the selective hydrogenation catalyst for carbon dioxide provided by the present invention affects the number of defects in the UiO-66(SO3H)2, thereby affecting the performance of the catalyst: a suitable amount of glacial acetic acid in the preparation method results in a moderate number of defects in the UiO-66(SO3H)2, allowing the Pt clusters and the exposed zirconium nodes at the defects to form a rich active interface. Too little glacial acetic acid results in too few defects, thus reducing the active interface and causing a decrease in both the yield and selectivity of methanol; too much glacial acetic acid results in too many defects, making product desorption difficult and reducing the yield of methanol.

[0143] A comparison of Examples 1-6 with Comparative Examples 1-3 reveals that the selective hydrogenation catalyst for carbon dioxide provided by this invention utilizes the zirconium nodes exposed at the defects of UiO-66(SO3H)2 and the sulfonated ligands to stabilize the small-sized Pt clusters. This results in the formation of a precise, abundant, and easily tunable active interface structure between the exposed zirconium nodes and the Pt clusters at the defects. Therefore, this catalyst exhibits superior performance in the selective hydrogenation of carbon dioxide compared to the traditional supported catalysts in the comparative examples. It overcomes the problem of difficulty in catalyzing the hydrogenation of carbon dioxide at low temperatures and demonstrates a certain activity in the selective hydrogenation of carbon dioxide to produce methanol at a low temperature of 60°C, as shown in the methanol space-time yield values ​​in Table 1, and exhibits high methanol selectivity.

[0144] (5) Catalytic stability test of carbon dioxide selective hydrogenation catalyst:

[0145] The catalyst Pt NCs@UiO-66(SO3H)2 provided in Example 1 underwent long-term catalytic stability testing. The catalytic testing was conducted continuously for 500 hours, maintaining a reaction temperature of 60°C, a pressure of 3 MPa, a gas flow rate of 10 mL / min, and continuous real-time sampling by a gas chromatograph. The stability test graph showing the change in methanol space-time yield of the catalyst Pt NCs@UiO-66(SO3H)2 provided in Example 1 as a function of reaction time is shown below. Figure 11 As shown; by Figure 11 It can be seen that the methanol space-time yield and selectivity remain unchanged within 500 h, indicating that the catalyst Pt NCs@UiO-66(SO3H)2 provided in Example 1 has excellent long-term stability.

[0146] After performing selective hydrogenation catalytic tests on the catalyst Pt NCs@UiO-66(SO3H)2 provided in Example 1, it was further tested using field emission transmission electron microscopy (Tecnai G2 F20 U-TWIN) and aberration-corrected transmission electron microscopy (FEI Titan Cubed Themis G2 300). The high-magnification, aberration-corrected, high-angle annular dark-field scanning electron microscope image of the reacted catalyst Pt NCs@UiO-66(SO3H)2 is shown below. Figure 12 As shown, the particle size distribution of the Pt clusters in the obtained catalyst Pt NCs@UiO-66(SO3H)2 after the reaction is as follows: Figure 13 As shown; by Figure 12 and Figure 13 It can be seen that after the selective hydrogenation catalytic reaction of carbon dioxide, the distribution and size of Pt clusters in the catalyst Pt NCs@UiO-66(SO3H)2 provided in Example 1 remain basically unchanged, with no agglomeration or sintering phenomenon, indicating that the catalyst has good stability.

[0147] After performing selective hydrogenation catalytic tests on the catalyst Pt NCs@UiO-66(SO3H)2 provided in Example 1, it was characterized by XRD using a Rigaku D / MAX-TTRIII spectrometer. The XRD pattern of the reacted catalyst Pt NCs@UiO-66(SO3H)2 is shown below. Figure 14 As shown; by Figure 14 It can be seen that after the selective hydrogenation catalytic reaction of carbon dioxide, the crystal structure of the catalyst Pt NCs@UiO-66(SO3H)2 provided in Example 1 remains unchanged, indicating that the catalyst has good stability.

[0148] The above description is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily conceived by those skilled in the art within the technical scope disclosed in the present invention fall within the protection and disclosure scope of the present invention.

Claims

1. A catalyst for the selective hydrogenation of carbon dioxide, characterized in that, The catalyst is Pt NCs@UiO-66(SO3H)2; The Pt NCs@UiO-66(SO3H)2 includes a metal-organic framework UiO-66(SO3H)2 and Pt clusters loaded on the metal-organic framework UiO-66(SO3H)2; The metal-organic framework UiO-66(SO3H)2 contains 10-50% molar content of sulfonated ligands and 50-90% molar content of non-sulfonated ligands; The Pt clusters are distributed in the channels of the metal-organic framework UiO-66(SO3H)2 and are fixed by zirconium nodes exposed at defects in the metal-organic framework UiO-66(SO3H)2 and sulfonic acid groups on the ligands. The method for preparing the catalyst includes the following steps: A Pt source, a metal-organic framework UiO-66(SO3H)2 and a solvent were mixed and then thermally reduced in a protective atmosphere containing reducing gases to obtain a Pt NCs@UiO-66(SO3H)2 catalyst. The mass ratio of the Pt source to the metal-organic framework UiO-66(SO3H)2 is (0.01~0.1):1; The Pt source includes any one or a combination of at least two of potassium tetrachloroplatinate, chloroplatinic acid, or platinum nitrate. The method for preparing the metal-organic framework UiO-66(SO3H)2 includes: The metal precursor, organic mixed ligand and organic solvent are mixed and then thermally synthesized to obtain UiO-66(SH)2. Then, the ligand is oxidized to obtain UiO-66(SO3H)2. The organic mixed ligands are terephthalic acid and 2,5-dimercaptoterephthalic acid; The ligand oxidation is performed by oxidizing the 2,5-dimercaptophthalic acid ligand in the thermally synthesized solid UiO-66(SH)2 to form a sulfonic acid group. The metal precursor is zirconium tetrachloride; The mixture also includes glacial acetic acid and water; The molar ratio of zirconium tetrachloride to glacial acetic acid in the mixture is 1:(25~175).

2. The catalyst according to claim 1, characterized in that, The particle size distribution of the Pt clusters is 0.6~2nm.

3. A method for preparing the catalyst according to claim 1 or 2, characterized in that, The preparation method includes: A Pt source, a metal-organic framework UiO-66(SO3H)2 and a solvent were mixed and then thermally reduced in a protective atmosphere containing reducing gases to obtain a Pt NCs@UiO-66(SO3H)2 catalyst. The mass ratio of the Pt source to the metal-organic framework UiO-66(SO3H)2 is (0.01~0.1):1; The Pt source includes any one or a combination of at least two of potassium tetrachloroplatinate, chloroplatinic acid, or platinum nitrate. The method for preparing the metal-organic framework UiO-66(SO3H)2 includes: The metal precursor, organic mixed ligand and organic solvent are mixed and then thermally synthesized to obtain UiO-66(SH)2. Then, the ligand is oxidized to obtain UiO-66(SO3H)2. The organic mixed ligands are terephthalic acid and 2,5-dimercaptoterephthalic acid; The ligand oxidation is performed by oxidizing the 2,5-dimercaptophthalic acid ligand in the thermally synthesized solid UiO-66(SH)2 to form a sulfonic acid group. The metal precursor is zirconium tetrachloride; The mixture also includes glacial acetic acid and water; The molar ratio of zirconium tetrachloride to glacial acetic acid in the mixture is 1:(25~175).

4. The preparation method according to claim 3, characterized in that, The mixing process includes: mixing a Pt source with a portion of the solvent to obtain a first mixture; mixing a metal-organic framework UiO-66(SO3H)2 with the remaining solvent to obtain a second mixture; adding the first mixture dropwise to the second mixture and then stirring.

5. The preparation method according to claim 3, characterized in that, The mixed Pt source, the metal-organic framework UiO-66(SO3H)2, and the solvent in the solvent are all water.

6. The preparation method according to claim 4, characterized in that, The solid-liquid ratio of the Pt source to the partial solvent is (2.1~9.6):1, and the unit of the solid-liquid ratio is mg / mL.

7. The preparation method according to claim 4, characterized in that, The solid-liquid ratio of the metal-organic framework UiO-66(SO3H)2 to the remaining solvent is (15~25):1, and the unit of the solid-liquid ratio is mg / mL.

8. The preparation method according to claim 4, characterized in that, The stirring process takes 10-15 hours.

9. The preparation method according to claim 4, characterized in that, After the stirring process is completed, the mixture is centrifuged and washed in sequence, and then placed in a vacuum oven to dry.

10. The preparation method according to claim 3, characterized in that, The volume concentration of reducing gas in the protective atmosphere is 5-15%.

11. The preparation method according to claim 3, characterized in that, The reducing gas is hydrogen.

12. The preparation method according to claim 3, characterized in that, The thermal reduction includes sequential heating and holding, with the heating rate being 1~5℃ / min, the final temperature being 180~220℃, and the holding time being 1.5~2.5h.

13. The preparation method according to claim 3, characterized in that, The organic solvent is N,N-dimethylformamide.

14. The preparation method according to claim 3, characterized in that, The volume of the organic solvent in the mixture is fixed at 45~55mL.

15. The preparation method according to claim 3, characterized in that, The molar ratio of zirconium tetrachloride to terephthalic acid in the mixture is 1:(0.6~0.9).

16. The preparation method according to claim 3, characterized in that, The molar ratio of terephthalic acid to 2,5-dimercaptoterephthalic acid in the mixture is (1~9):

1.

17. The preparation method according to claim 3, characterized in that, The molar ratio of zirconium tetrachloride to water in the mixture is 1:(2~4).

18. The preparation method according to claim 3, characterized in that, The thermal synthesis is carried out at a temperature of 110~130℃ for 20~28h.

19. The preparation method according to claim 3, characterized in that, After the thermal synthesis is completed, the sample is centrifuged and washed in sequence, and then dried in a vacuum oven to obtain solid UiO-66(SH)2.

20. The preparation method according to claim 3, characterized in that, The oxidation process includes: dispersing the solid UiO-66(SH)2 obtained after thermal synthesis in a 15-45% hydrogen peroxide aqueous solution and stirring the reaction.

21. The preparation method according to claim 20, characterized in that, The solid-liquid ratio of the thermally synthesized solid UiO-66(SH)2 to the hydrogen peroxide solution is (8~12):1, and the unit of the solid-liquid ratio is mg / mL.

22. The preparation method according to claim 20, characterized in that, The stirring reaction time is 20-28 hours.

23. The preparation method according to claim 20, characterized in that, The stirring reaction was carried out under light-protected conditions.

24. The preparation method according to claim 3, characterized in that, The preparation method includes: (1) Zirconium tetrachloride, glacial acetic acid, water, terephthalic acid, 2,5-dimercaptoterephthalic acid and 45~55 mL of N,N-dimethylformamide were mixed and then thermally synthesized at 110~130℃ for 20~28 h. After centrifugation, washing and drying, solid UiO-66(SH)2 was obtained. The obtained solid UiO-66(SH)2 was dispersed in 15~45% hydrogen peroxide aqueous solution. The solid-liquid ratio of solid UiO-66(SH)2 to hydrogen peroxide aqueous solution was (8~12):

1. The unit of the solid-liquid ratio was mg / mL. Then, the reaction was carried out in the dark for 20~28 h with stirring to obtain UiO-66(SO3H)2. The molar ratio of zirconium tetrachloride to terephthalic acid in the mixture is 1:(0.6~0.9), the molar ratio of terephthalic acid to 2,5-dimercaptoterephthalic acid is (1~9):1, the molar ratio of zirconium tetrachloride to glacial acetic acid is 1:(25~175), and the molar ratio of zirconium tetrachloride to water is 1:(2~4). (2) Mix Pt source with part of solvent water to obtain a first mixture; mix UiO-66(SO3H)2 with the remaining solvent water to obtain a second mixture; add the obtained first mixture to the obtained second mixture dropwise, and then stir for 10~15h. After centrifugation, washing and drying, a solid powder is obtained. The mass ratio of the Pt source to UiO-66(SO3H)2 is (0.01~0.1):1, the solid-liquid ratio of the Pt source to the partial solvent water is (2.1~9.6):1, and the solid-liquid ratio of UiO-66(SO3H)2 to the remaining solvent water is (15~25):

1. The units of the solid-liquid ratios are all mg / mL. (3) The solid powder obtained in step (2) is heated to 180-220°C at a rate of 1-5°C / min in a protective atmosphere with a hydrogen volume concentration of 5-15% and then kept at the temperature for 1.5-2.5h to obtain Pt NCs@UiO-66(SO3H)2 catalyst.

25. An application of the catalyst according to claim 1 or 2, characterized in that, The catalyst is used to catalyze the hydrogenation reaction of carbon dioxide.

Citation Information

Patent Citations

  • Synthetic method and application of supported NH2-UiO-66 hydrogenation catalyst

    CN108097315A

  • Preparation method and application of high-stability solid acid based on metal organic framework

    CN112742481A

  • Catalytic hydrogenation catalyst and preparation method and application thereof

    CN112742482A

  • Preparation method of amino-functionalized UiO-66 loaded platinum-cobalt bimetallic nano-alloy catalyst

    CN116786169A