A method for washing-free treatment of high-purity silicon carbide powder
By combining a tungsten carbide crusher with oxygen heating, the problems of impurity introduction and cleaning in the preparation of silicon carbide powder in the existing technology have been solved, realizing the preparation of high-purity silicon carbide powder with high efficiency and low cost, and improving the quality and yield of single crystals.
Patent Information
- Application Number
- CN202410617603.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-17
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-05-17
AI Technical Summary
Existing technologies involve cumbersome steps in the preparation of silicon carbide powder, such as magnetic separation, rinsing, and acid washing, which can easily introduce metallic impurities and make it difficult to completely remove fine carbides, affecting the quality and yield of single crystal crystallization.
A tungsten carbide crusher is used to crush silicon carbide lumps, which are then microwave-heated in an oxygen-containing gas atmosphere to remove impurities by reacting oxygen with the tungsten carbide. The material is then sieved using a polyurethane screen to avoid additional cleaning steps.
The preparation of high-purity silicon carbide powder with low metal impurity content has been achieved, simplifying the processing flow and improving the preparation efficiency and crystal growth yield.
Abstract
Description
Technical Field
[0001] This invention belongs to the field of silicon carbide crystal material preparation technology, and particularly relates to a washing-free treatment method for high-purity silicon carbide powder. Background Technology
[0002] Silicon carbide (SiC), as a third-generation semiconductor material, possesses significant advantages over silicon-based semiconductor materials and is widely used in power semiconductor devices and microwave radio frequency devices. Currently, silicon carbide single crystals are synthesized from silicon carbide powder using the PVT (physical vapor transport) method. The key to this method lies in the growth environment and the purity of the SiC powder, especially since the purity of the SiC powder directly affects the crystal quality and electrical properties of the single crystal.
[0003] Currently, SiC powder is mainly prepared using the high-temperature solid-state method. Solid carbon powder and silicon powder are used as raw materials, and SiC is generated through continuous reaction at high temperatures. However, the resulting silicon carbide is in block form with a large number of carbide inclusions. It requires crushing, magnetic separation, rinsing, acid washing, and sieving to obtain silicon carbide powder of the desired particle size. This process is cumbersome and easily introduces metallic impurities during crushing, reducing the purity of the silicon carbide powder. Secondly, since the synthesis of silicon carbide requires temperatures above 2000℃, a large amount of carbide and unreacted carbon powder are generated at high temperatures. These fine carbides and carbon powder are difficult to clean completely and can form inclusions during crystal growth, reducing the yield of crystal growth. Summary of the Invention
[0004] The purpose of this invention is to provide a washing-free treatment method for high-purity silicon carbide powder. The treatment method of this invention does not require magnetic separation, rinsing, acid washing and other steps, and has a low content of surface metal impurities. It can effectively remove fine carbides in the powder and improve the yield of crystal growth.
[0005] This invention provides a washing-free treatment method for high-purity silicon carbide powder, comprising the following steps:
[0006] A) The silicon carbide block material is crushed using a tungsten carbide crusher to obtain silicon carbide powder;
[0007] B) Spread silicon carbide powder evenly into a quartz disc and heat it in an oxygen-containing gas atmosphere to obtain high-purity silicon carbide powder.
[0008] Preferably, the thickness of the silicon carbide powder in the quartz disk is <10mm.
[0009] Preferably, in step B), the temperature is first raised to 800-850°C and held for 0.5-2 hours, and then raised to 1000-1100°C and held for 0.5-1 hour.
[0010] Preferably, the temperature is increased from 800-850℃ to 1000-1100℃ within 20-40 minutes.
[0011] Preferably, the oxygen-containing gas is high-purity oxygen.
[0012] Preferably, in step B), the flow rate of the oxygen-containing gas is 800–1200 sccm.
[0013] Preferably, step B) uses a microwave heating device for heating.
[0014] Preferably, after heating, the material is cooled to room temperature and then sieved using a polyurethane sieve to obtain high-purity silicon carbide powder.
[0015] This invention provides a method for washing-free processing of high-purity silicon carbide powder, comprising the following steps: A) crushing silicon carbide lumps using a tungsten carbide crusher to obtain silicon carbide granules; B) spreading the silicon carbide granules evenly into a quartz disc and heating them in an oxygen-containing gas atmosphere to obtain high-purity silicon carbide powder.
[0016] Compared with existing technologies, the beneficial effects of this technical solution are as follows:
[0017] 1. The present invention incorporates a single type of metal impurity during crushing, resulting in a lower metal impurity content on the surface of silicon carbide powder compared to existing technologies.
[0018] 2. The method of the present invention is simple and efficient: The washing-free method of the present invention processes high-purity silicon carbide powder without the need for magnetic separation, rinsing, acid washing and other steps. Compared with the prior art, the method of the present invention improves the preparation efficiency and reduces the production cost.
[0019] 3. The method in this invention can effectively remove fine carbides from silicon carbide powder and increase the yield of crystal growth;
[0020] In summary, compared with existing technologies, this invention has advantages such as a simple and efficient preparation method, higher purity, and better crystal growth effect. This invention can improve the processing efficiency and quality of silicon carbide powder. Detailed Implementation
[0021] This invention provides a washing-free treatment method for high-purity silicon carbide powder, comprising the following steps:
[0022] A) The silicon carbide block material is crushed using a tungsten carbide crusher to obtain silicon carbide powder;
[0023] B) Spread silicon carbide powder evenly into a quartz disc and heat it in an oxygen-containing gas atmosphere to obtain high-purity silicon carbide powder.
[0024] The present invention first uses a tungsten carbide crusher to crush the synthesized block silicon carbide material to obtain granular silicon carbide powder required for crystal growth.
[0025] In this invention, the silicon carbide block material can be any commonly used silicon carbide block material in the art, and this invention does not impose any special limitations on it.
[0026] The present invention preferably uses a crusher made of tungsten carbide. Tungsten carbide has a hardness similar to that of diamond, with a Mohs hardness of 9 to 9.5. It experiences less wear during crushing, and the impurities it contains are singular, with WC as the main component.
[0027] After obtaining silicon carbide powder, the present invention lays the silicon carbide powder flat in a quartz dish.
[0028] In this invention, the loading container for silicon carbide powder is a quartz disk, and the heat resistance temperature of the quartz material is 1750℃; the loading thickness of the silicon carbide powder is preferably <10mm, and the processing purity will decrease if the thickness is >10mm.
[0029] In this invention, a quartz disc containing silicon carbide powder is placed into a heating device, and oxygen-containing gas is introduced to carry out a heating reaction.
[0030] In this invention, the heating device is preferably a microwave heating device, that is, the heating reaction is a microwave heating reaction; the heating reaction is preferably divided into two stages, the heating temperature of the first stage is preferably 800-850℃, more preferably 810-840℃, such as 800℃, 805℃, 810℃, 815℃, 820℃, 825℃, 830℃, 835℃, 840℃, 845℃, 850℃, preferably a range of values with any of the above values as the upper or lower limit; the holding time of the first stage of heating is preferably 0.5-2 hours, more preferably 1-1.5 hours; in this heating stage, high-purity oxygen is introduced to react with the fine tungsten carbide impurities on the surface of the silicon carbide powder. During this process, the tungsten carbide impurities introduced by the crusher made of tungsten carbide material also react with oxygen, such as WC + O2 = WO2 + CO2.
[0031] In this invention, high-purity oxygen is continuously introduced from the start of heating until the heating treatment is completed. The flow rate of the high-purity oxygen is preferably 800-1200 sccm, more preferably 900-1100 sccm, and most preferably 1000-1050 sccm.
[0032] After the first stage of heating is completed, the temperature is raised to 1000-1100°C within 20-40 minutes, preferably within 25-30 minutes, for the second stage of heating. The main purpose of this stage of heating is to remove the WO2 produced in the first stage and allow it to volatilize at high temperature.
[0033] In this invention, the heating temperature in the second stage is preferably 1000-1100℃, more preferably 1050-1100℃, such as 1000℃, 1010℃, 1020℃, 1030℃, 1040℃, 1050℃, 1060℃, 1070℃, 1080℃, 1090℃, 1100℃, preferably a range of values with any of the above values as the upper or lower limit; the heating holding time is preferably 0.5-1 hour.
[0034] After heating is complete and the material has cooled to room temperature, the silicon carbide powder is removed and sieved using a polyurethane sieve to obtain high-purity silicon carbide powder. Using a polyurethane sieve helps to avoid contamination during the sieving process.
[0035] This invention provides a no-washing treatment method for high-purity silicon carbide powder, comprising the following steps: A) crushing silicon carbide lumps using a tungsten carbide crusher to obtain silicon carbide granules; B) spreading the silicon carbide granules evenly into a quartz disc and heating them in an oxygen-containing gas atmosphere to obtain high-purity silicon carbide powder. Compared with the prior art, this technical solution mainly solves the following technical problems: 1. The treatment method in this invention eliminates the need for magnetic separation, rinsing, and acid washing after crushing the synthesized silicon carbide raw material, and has a low content of surface metal impurities, thus improving the processing efficiency and quality of silicon carbide powder; 2. The treatment method in this invention can effectively remove fine carbides from the powder, improving the yield of crystal growth.
[0036] To further illustrate the present invention, the following detailed description of a washing-free treatment method for high-purity silicon carbide powder provided by the present invention is provided in conjunction with embodiments, but it should not be construed as limiting the scope of protection of the present invention.
[0037] Example 1
[0038] Step 1: The silicon carbide blocks obtained by high-temperature synthesis are fed into a tungsten carbide crusher for crushing;
[0039] Step 2: Spread the crushed silicon carbide powder evenly in a quartz dish;
[0040] Step 3: Place the quartz disk containing silicon carbide powder into a microwave heater and introduce oxygen to carry out the heating reaction. Control the temperature at 800℃, introduce high-purity oxygen at 1000 SCCM, maintain for 1 hour, then increase the temperature to 1100℃ over 30 minutes and maintain for 1 hour.
[0041] Step 4: After cooling, remove the powder and sieve it using a polyurethane sieve to obtain high-purity, clean silicon carbide powder.
[0042] Step 5: The content of metallic impurities in the raw materials crushed by the crusher is <120ppb.
[0043] Step 6: Using the obtained high-purity silicon carbide powder, 8 silicon carbide crystals were grown. The proportion of wafers with less than 0.05% inclusions per wafer was 92%, while the proportion of wafers with less than 0.05% inclusions per wafer was 82.4% when the raw material was grown by ordinary cleaning method. The yield was better than that of raw material processed by cleaning method.
[0044] Example 2
[0045] Step 1: The silicon carbide blocks obtained by high-temperature synthesis are fed into a tungsten carbide crusher for crushing;
[0046] Step 2: Spread the crushed silicon carbide powder evenly in a quartz dish;
[0047] Step 3: Place the quartz disk containing silicon carbide powder into a microwave heater and introduce oxygen to carry out the heating reaction. Control the temperature at 850℃ while simultaneously introducing high-purity oxygen at 1000 SCCM, maintain for 1 hour, then increase the temperature to 1000℃ over 30 minutes and maintain for 1 hour.
[0048] Step 4: After cooling, remove the powder and sieve it using a polyurethane sieve to obtain high-purity, clean silicon carbide powder.
[0049] Step 5: The content of metallic impurities in the raw material crushed by the tungsten carbide crusher is <120ppb.
[0050] Step 6: Use the obtained high-purity silicon carbide powder to grow 8 silicon carbide crystals.
[0051] The inclusion content in silicon carbide crystals is detected by slicing. Inclusions are caused by impurities in the raw material and are unavoidable defects. However, they are graded as <0.05% / wafer and ≥0.05%<5% / wafer. The lower the percentage, the fewer the inclusions. Therefore, the quality of silicon carbide crystals can be evaluated by measuring the proportion of inclusions in the wafer. Generally, fewer inclusions are considered to indicate better silicon carbide crystal quality. In this embodiment, among all inclusions, the proportion of inclusions <0.05% in slicing is 92.5%, which is better than that of raw materials processed by cleaning.
[0052] Comparative Example 1
[0053] Step 1: The silicon carbide blocks obtained from high-temperature synthesis are fed into a tungsten carbide crusher for crushing;
[0054] Step 2: Spread the silicon carbide powder obtained from the crusher evenly in a quartz dish; place the quartz dish containing the silicon carbide powder into a microwave heater, and introduce oxygen to carry out the heating reaction. Control the temperature at 600℃, introduce high-purity oxygen at 1000 SCCM, maintain for 1 hour, then raise the temperature to 1000℃ in 30 minutes and maintain for 1 hour;
[0055] Step 3: After the raw material has cooled, remove it and sieve it using a polyurethane sieve to obtain high-purity and clean silicon carbide powder;
[0056] Step 5: The processed silicon carbide powder was tested, and the metal impurity content of the raw material crushed by the tungsten carbide crusher was measured to be 204.4 ppb.
[0057] Step 6: Use the obtained high-purity silicon carbide powder to grow 8 silicon carbide crystals. The cross-section analysis showed that the percentage of inclusions <0.05% was 89.3%.
[0058] Comparative Example 2
[0059] Step 1: The silicon carbide blocks obtained by high-temperature synthesis are fed into a manganese steel crusher for crushing;
[0060] Step 2: The raw materials crushed by the manganese steel crusher are pickled with 15% sulfuric acid and then dried.
[0061] Step 3: After the raw material has cooled, remove it and sieve it using a polyurethane sieve to obtain high-purity and clean silicon carbide powder;
[0062] Step 4: The processed silicon carbide powder was tested, and the content of metallic impurities on the surface of the raw material crushed by the manganese steel crusher was measured to be 630.56 ppb.
[0063] Step 5: Use the obtained high-purity silicon carbide powder to grow 8 silicon carbide crystals. The proportion of wafers with less than 0.05% inclusions was 83.2%.
[0064] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.
Claims
1. A method for washing-free treatment of high-purity silicon carbide powder, comprising the following steps: A) The silicon carbide block material is crushed using a tungsten carbide crusher to obtain silicon carbide powder; B) Spread the silicon carbide powder evenly into a quartz disk and heat it using a microwave heating device in an oxygen-containing gas atmosphere. First, raise the temperature to 800~850℃ and hold for 0.5~2 hours. Then, within 20~40 minutes, raise the temperature to 1000~1100℃ and hold for 0.5~1 hours to obtain high-purity silicon carbide powder.
2. The method for washing-free treatment of high-purity silicon carbide powder according to claim 1, characterized in that, The thickness of the silicon carbide powder in the quartz disk is <10mm.
3. The method for washing-free treatment of high-purity silicon carbide powder according to claim 1, characterized in that, The oxygen-containing gas is high-purity oxygen.
4. The method for washing-free treatment of high-purity silicon carbide powder according to claim 3, characterized in that, In step B), the flow rate of the oxygen-containing gas is 800~1200 sccm.
5. The no-wash treatment method according to claim 1, characterized in that, After heating, the material is cooled to room temperature and then sieved using a polyurethane sieve to obtain high-purity silicon carbide powder.