Method for preparing Ti3Al alloy coated steel sheet by magnetron sputtering, coated steel sheet

By using magnetron sputtering to deposit a Ti₃Al alloy coating on the surface of hot-formed steel, the oxidation and corrosion problems of hot-formed steel are solved, achieving a highly efficient and environmentally friendly anti-corrosion effect and extending the service life of hot-formed steel.

CN118639201BActive Publication Date: 2026-11-20SHOUGANG JINGTANG IRON & STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410891292.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2026-11-20
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

Existing hot-formed steel is prone to oxidation and corrosion during service. Zinc-based coatings result in the waste of zinc resources, while aluminum-silicon coatings have high production costs and poor processing plasticity. There is an urgent need to develop a new, efficient, and green anti-corrosion method.

Method used

A Ti₃Al alloy coating is deposited on the surface of hot-formed steel using magnetron sputtering technology. Surface oxides and oil are removed through pretreatment, and the oxidation and corrosion resistance of Ti₃Al alloy is utilized to form a Ti₃Al alloy coating with a thickness of 1μm to 3μm.

Benefits of technology

It significantly improves the corrosion resistance of hot-formed steel, reduces production costs, avoids the defects of traditional methods, and extends service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118639201B_ABST
    Figure CN118639201B_ABST
Patent Text Reader

Abstract

The application provides a method for preparing a Ti3Al alloy plated steel sheet by magnetron sputtering and the plated steel sheet, and belongs to the alloy plating field.The method comprises the following steps: pretreating a hot forming steel bare plate to obtain a pretreated bare plate; taking Ti3Al alloy as a target material, and performing magnetron sputtering treatment on the pretreated bare plate to form a Ti3Al alloy-containing plating layer on at least part of the surface of the pretreated bare plate, thereby obtaining a Ti3Al alloy plated steel sheet.Through the pretreatment of the hot forming steel bare plate, the surface oxides, dust and oil stains of the bare plate are removed, so that the magnetron sputtering treatment is not affected; and through the adoption of the magnetron sputtering technology, the Ti3Al alloy plating film with strong oxidation resistance and corrosion resistance is deposited on the surface of the hot forming steel bare plate, so that the corrosion resistance of the hot forming steel is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of alloy coating technology, and in particular to a method for preparing Ti3Al alloy coated steel plates using magnetron sputtering, and the coated steel plates. Background Technology

[0002] Currently, the pressure to reduce carbon emissions in the transportation sector is increasing, leading to a new surge in the research and application of lightweight materials. Hot-formed steel, with its high strength and light weight, is favored by the industry and is widely used in the manufacture of automotive structural components, thus boosting the development of the automotive industry. Based on the application of hot-formed steel, while ensuring the safety and reliability of the vehicle body, it effectively reduces the vehicle's weight, meeting the stringent requirements of the automotive industry for low fuel consumption, low emissions, and safety.

[0003] Currently, the common applications of hot-formed steel include three types: bare sheet, zinc-based coating, and aluminum-silicon coating. Bare sheet is prone to surface oxidation and corrosion during service, severely impacting component lifespan. Zinc-based coatings involve zinc evaporation during production, resulting in zinc ash and dross, wasting zinc resources and affecting the surface quality of the strip. Aluminum-silicon coatings have high production costs and poor processing plasticity. Therefore, there is an urgent need to develop a new, efficient, and environmentally friendly corrosion-resistant method to improve the corrosion protection of hot-formed steel. Summary of the Invention

[0004] This application provides a method for preparing Ti3Al alloy coated steel sheet using magnetron sputtering, and the coated steel sheet, to solve the following technical problem: how to improve the corrosion resistance of hot-formed steel.

[0005] In a first aspect, this application provides a method for preparing Ti3Al alloy-coated steel plates using magnetron sputtering, the method comprising:

[0006] Hot-formed steel sheets are pretreated to obtain pretreated sheets;

[0007] Using Ti3Al alloy as the target material, the pretreated bare plate is subjected to magnetron sputtering to form a Ti3Al alloy-containing coating on at least a portion of the surface of the pretreated bare plate, thereby obtaining a Ti3Al alloy-coated steel plate.

[0008] Optionally, the step of using Ti3Al alloy as the target material to perform magnetron sputtering treatment on the pretreated bare plate includes:

[0009] The pretreated bare plate is placed in a vacuum chamber, and a magnetron sputtering Ti3Al alloy target is provided in the vacuum chamber. The distance between the pretreated bare plate and the magnetron sputtering Ti3Al alloy target is 120mm to 160mm.

[0010] The pretreated bare plate was treated with the magnetron sputtering Ti3Al alloy target.

[0011] Optionally, the step of treating the pretreated bare plate with the magnetron sputtering Ti3Al alloy target includes:

[0012] Adjust the vacuum level of the vacuum chamber to the first set vacuum level;

[0013] Argon gas is introduced into the vacuum chamber with a first set vacuum degree, and the vacuum degree is adjusted to a second vacuum degree. Then, the pre-treated bare plate is cleaned with a gas ion source to obtain a clean bare plate.

[0014] Adjust the vacuum level of the vacuum chamber to the third set vacuum level, and adjust the bias voltage of the clean bare plate to the set bias voltage;

[0015] Ti3Al alloy was magnetron sputtered and deposited on the clean bare plate using a DC power supply.

[0016] Optionally, the bias voltage is set to -80V to -120V.

[0017] Optionally, the first set vacuum degree is <5×10 -4 Pa, the second vacuum degree is 0.25Pa to 0.35Pa, the third set vacuum degree is 0.75Pa to 0.85Pa, and the argon gas flow rate is 60sccm to 80sccm.

[0018] Optionally, the gas ion source cleaning includes the following parameters: rotation speed of the rotating frame is 3r / min to 6r / min, voltage is 720V to 780V, current is 0.2A to 0.4A, and cleaning time is 25min to 35min.

[0019] Optionally, the magnetron sputtering includes the following parameters: power of 600W to 750W and sputtering time of 70min to 100min.

[0020] Optionally, the pretreatment of the hot-formed steel sheet to obtain a pretreated sheet includes:

[0021] The hot-formed steel bare plate was polished step by step using sandpaper with grits of 200#, 1000# and 3000#, followed by ultrasonic cleaning and drying to obtain a pre-treated bare plate; the ultrasonic cleaning time was 25 min to 35 min.

[0022] In a second aspect, this application provides a Ti3Al alloy-coated steel sheet prepared by the method described in any one embodiment of the first aspect, wherein the Ti3Al alloy-coated steel sheet comprises a hot-formed steel bare sheet and a Ti3Al alloy coating covering at least a portion of the surface of the hot-formed steel bare sheet, and the thickness of the Ti3Al alloy coating is 1 μm to 3 μm.

[0023] Optionally, the corrosion current density of the Ti3Al alloy-coated steel plate is ≤6.5×10⁻⁶. -7 A / cm 2 .

[0024] The technical solutions provided in this application have the following advantages compared with the prior art:

[0025] This application provides a method for preparing Ti3Al alloy-coated steel sheets using magnetron sputtering, comprising: pre-treating a hot-formed steel bare sheet to obtain a pre-treated bare sheet; using Ti3Al alloy as a target material, performing magnetron sputtering treatment on the pre-treated bare sheet to form a Ti3Al alloy-containing coating on at least a portion of the surface of the pre-treated bare sheet, thereby obtaining a Ti3Al alloy-coated steel sheet. By pre-treating the hot-formed steel bare sheet, oxides, dust, and oil stains on the surface of the bare sheet are removed, avoiding any impact on the magnetron sputtering treatment; by employing magnetron sputtering technology to deposit a Ti3Al alloy coating with strong oxidation resistance and corrosion resistance onto the surface of the hot-formed steel bare sheet, the corrosion resistance of the hot-formed steel is improved. Attached Figure Description

[0026] The accompanying drawings, which are incorporated in and form part of this specification, illustrate embodiments consistent with this application and, together with the description, serve to explain the principles of this application.

[0027] To more clearly illustrate the technical solutions in the embodiments of this application or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0028] Figure 1 A flowchart illustrating a method for preparing Ti3Al alloy-coated steel plates using magnetron sputtering, as provided in this application embodiment;

[0029] Figure 2 The diagram shows the Ti3Al alloy coated steel sheet (a), the pretreated bare sheet (b), and the aluminum-silicon coated steel sheet (c) provided in Embodiment 1 and Comparative Examples 1 and 2 of this application.

[0030] Figure 3 The polarization curves of the electrochemical corrosion test provided in Example 1 and Comparative Examples 1 and 2 of this application. Detailed Implementation

[0031] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions of the embodiments of this application will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this application, not all embodiments. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of this application.

[0032] Various embodiments of this application may exist in the form of a range; it should be understood that the description in the form of a range is merely for convenience and brevity and should not be construed as a hard limitation on the scope of this application; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within that range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., and single numbers within the range, such as 1, 2, 3, 4, 5, and 6, regardless of the range. Furthermore, whenever a numerical range is referred to herein, it means including any referenced number (fraction or integer) within the referred range.

[0033] Furthermore, in the description of this application, the terms "comprising," "including," etc., mean "including but not limited to." In this document, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this document, "and / or" describes the relationship between related objects, indicating that three relationships can exist; for example, A and / or B can represent: A alone, A and B simultaneously, or B alone. A and B can be singular or plural. In this document, "at least one" means one or more, and "more than" means two or more. "At least one," "at least one of the following," or similar expressions refer to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c" or "at least one of a, b, and c" can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, and c can be a single or multiple.

[0034] Unless otherwise specified, all raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.

[0035] Titanium and titanium alloys, with their excellent characteristics such as low density, high strength, oxidation resistance, and corrosion resistance, are widely used in shipbuilding, marine, and chemical industries. Titanium and titanium alloys exhibit high corrosion resistance to acids, alkalis, and salts in marine and marine atmospheric environments, making them ideal protective materials that can meet the performance requirements of components requiring "lighter, stronger, and more heat-resistant" materials. Among them, Ti3Al alloy has a lower density and stronger corrosion resistance than conventional pure titanium and titanium alloys. Therefore, to address the corrosion problem on the surface of hot-formed steel, a Ti3Al alloy coating can be deposited on the surface of the hot-formed steel to improve the corrosion resistance of the substrate.

[0036] Magnetron sputtering is a type of physical vapor deposition (PVD). It features simple equipment, ease of control, and advantages such as high deposition speed, dense and uniform coating, good adhesion, and large coating area. Its principle involves using high-energy particles or particle beams to bombard the target surface under the combined influence of an electric and magnetic field in a vacuum environment. This energy exchange causes target atoms or molecules to escape from the surface. The process of these escaped target atoms or molecules ultimately depositing as a film on the substrate surface is called magnetron sputtering coating. This technology is widely used in the machining industry, effectively improving the surface hardness, toughness, wear resistance, and corrosion resistance of substrates, thereby significantly extending the service life of coated products.

[0037] This application employs magnetron sputtering technology to deposit a Ti3Al alloy coating with strong oxidation and corrosion resistance onto the surface of a hot-formed steel bare plate, thereby enhancing its corrosion resistance.

[0038] Figure 1 This is a flowchart illustrating a method for preparing Ti3Al alloy-coated steel plates using magnetron sputtering, as provided in an embodiment of this application.

[0039] Please see Figure 1 This application provides a method for preparing Ti3Al alloy-coated steel plates using magnetron sputtering, the method comprising:

[0040] S1. Pre-treat the hot-formed steel sheet to obtain a pre-treated bare sheet;

[0041] In some embodiments, the pretreatment of the hot-formed steel sheet to obtain a pretreated sheet includes:

[0042] The hot-formed steel bare plate was polished step by step using sandpaper with grits of 200#, 1000# and 3000#, followed by ultrasonic cleaning and drying to obtain a pre-treated bare plate; the ultrasonic cleaning time was 25 min to 35 min.

[0043] The bare hot-formed steel sheet is simply sanded with sandpaper to remove oxides from the surface through progressive sanding. The sheet is then placed in an acetone solution and cleaned using an ultrasonic cleaner to remove dust and oil. Afterward, the ultrasonically cleaned hot-formed steel sheet is rinsed with running water and dried with a hairdryer.

[0044] S2. Using Ti3Al alloy as the target material, the pretreated bare plate is subjected to magnetron sputtering to form a Ti3Al alloy-containing coating on at least a portion of the surface of the pretreated bare plate, thereby obtaining a Ti3Al alloy-coated steel plate.

[0045] In some embodiments, the process of using Ti3Al alloy as a target material to perform magnetron sputtering treatment on the pretreated bare plate includes: placing the pretreated bare plate in a vacuum chamber, wherein a magnetron sputtering Ti3Al alloy target is provided in the vacuum chamber, and the distance between the pretreated bare plate and the magnetron sputtering Ti3Al alloy target is 120mm to 160mm; and treating the pretreated bare plate with the magnetron sputtering Ti3Al alloy target.

[0046] It should be noted that the distance between the pretreated bare substrate and the magnetron sputtering Ti3Al alloy target is the target-substrate distance. Controlling the target-substrate distance to 120mm to 160mm can avoid both high surface roughness of the coating and excessively low deposition rate. For example, the distance between the pretreated bare substrate and the magnetron sputtering Ti3Al alloy target can be 120mm, 130mm, 140mm, 150mm, 155mm, 160mm, etc.

[0047] In some embodiments, the process of treating the pretreated bare plate with the magnetron sputtering Ti3Al alloy target includes: adjusting the vacuum degree of the vacuum chamber to a first set vacuum degree; introducing argon gas into the vacuum chamber with the first set vacuum degree and adjusting the vacuum degree to a second vacuum degree, then cleaning the pretreated bare plate with a gas ion source to obtain a clean bare plate; adjusting the vacuum degree of the vacuum chamber to a third set vacuum degree and adjusting the bias voltage of the clean bare plate to a set bias voltage; and using a DC power supply to magnetron sputter and deposit Ti3Al alloy on top of the clean bare plate.

[0048] In some implementations, the set bias voltage is -80V to -120V.

[0049] It should be noted that setting the bias voltage to -80 to -120V can provide an additional electric field and improve the ionization rate. For example, the bias voltage can be -80V, -90V, -100V, -110V, -120V, etc.

[0050] In some embodiments, the first set vacuum degree is <5×10 -4Pa, the second vacuum degree is 0.25Pa to 0.35Pa, the third set vacuum degree is 0.75Pa to 0.85Pa, and the argon gas flow rate is 60sccm to 80sccm.

[0051] It should be noted that the introduced argon gas is ionized into argon ions, which then bombard the target surface, causing the deposited atoms to overflow. For example, the argon gas flow rate can be 60 sccm, 65 sccm, 70 sccm, 75 sccm, 80 sccm, etc.

[0052] In some embodiments, the gas ion source cleaning includes the following parameters: the rotation speed of the rotating frame is 3 r / min to 6 r / min, the voltage is 720V to 780V, the current is 0.2A to 0.4A, and the cleaning time is 25min to 35min.

[0053] It should be noted that the pre-treated bare board is fixed in a substrate fixture of a specially sized specification. The substrate fixture is connected to the rotating frame. Therefore, controlling the rotation speed of the rotating frame is essentially controlling the rotation speed of the pre-treated bare board. For example, the rotation speed of the rotating frame can be 3 r / min, 4 r / min, 5 r / min, 6 r / min, etc., the voltage can be 720V, 730V, 740V, 750V, 760V, 770V, 780V, etc., the current can be 0.2A, 0.25A, 0.30A, 0.35A, 0.4A, etc., and the cleaning time can be 25min, 28min, 30min, 32min, 35min, etc.

[0054] In some embodiments, the magnetron sputtering includes the following parameters: power of 600W to 750W and sputtering time of 70min to 100min.

[0055] It should be noted that controlling the parameters of magnetron sputtering ensures the escape of titanium and aluminum atoms while avoiding uneven coating. For example, the power can be 600W, 650W, 700W, 750W, etc., and the sputtering time can be 70min, 75min, 80min, 85min, 90min, 95min, 100min, etc.

[0056] In some embodiments, the method further includes: after the sputtering time is over, waiting for the temperature to cool to room temperature, closing the gate valve, molecular pump, and mechanical pump, removing the sample, and obtaining a Ti3Al alloy coated steel plate.

[0057] This application provides a Ti3Al alloy coated steel sheet, which includes a hot-formed steel bare sheet and a Ti3Al alloy coating covering at least a portion of the surface of the hot-formed steel bare sheet, wherein the thickness of the Ti3Al alloy coating is 1μm to 3μm.

[0058] It should be noted that Ti3Al alloy coatings can be used not only for hot-formed steel but also for other similar types of steel. A schematic diagram of Ti3Al alloy-coated steel sheets can be found here. Figure 2 .

[0059] By controlling the thickness of the Ti3Al alloy coating to be between 1μm and 3μm, strong corrosion resistance is ensured while reducing production costs. For example, the thickness of the Ti3Al alloy coated steel sheet can be 1μm, 1.5μm, 2μm, 2.5μm, 3μm, etc.

[0060] In some embodiments, the corrosion current density of the Ti3Al alloy-coated steel sheet is ≤6.5×10⁻⁶. -7 A / cm 2 .

[0061] The magnetron sputtering of Ti3Al alloy coatings significantly improves the corrosion resistance of hot-formed steel due to the excellent corrosion resistance of titanium alloys themselves. For example, the corrosion current density of the Ti3Al alloy-coated steel sheet can be 1×10⁻⁶. - 7 A / cm 2 2×10 -7 A / cm 2 3×10 -7 A / cm 2 4×10 -7 A / cm 2 5×10 -7 A / cm 2 6×10 -7 A / cm 2 6.5×10 -7 A / cm 2 wait.

[0062] The Ti3Al alloy coated steel sheet is realized based on the above-described preparation method of Ti3Al alloy coated steel sheet. The specific steps of the preparation method of Ti3Al alloy coated steel sheet can be referred to the above embodiments. Since the Ti3Al alloy coated steel sheet adopts some or all of the technical solutions of the above embodiments, it has at least all the beneficial effects brought about by the technical solutions of the above embodiments, which will not be elaborated here.

[0063] The present application is further illustrated below with reference to specific embodiments. It should be understood that these embodiments are for illustrative purposes only and are not intended to limit the scope of the application. Experimental methods in the following embodiments that do not specify specific conditions are generally determined according to industry standards. If there is no corresponding industry standard, then common international standards, conventional conditions, or conditions recommended by the manufacturer are followed.

[0064] Example 1

[0065] This embodiment provides a method for preparing Ti3Al alloy-coated steel plates using magnetron sputtering, comprising the following steps:

[0066] (1) The hot-formed steel bare plate (the size of the hot-formed steel bare plate is 100mm×70mm×1.4mm) is simply sanded with sandpaper of grits 200#, 1000# and 3000#. After sanding with sandpaper of different grits, the oxides on the surface of the bare plate can be removed. Then, the bare plate is placed in acetone solution and cleaned with an ultrasonic cleaner for 30 minutes to remove dust and oil stains from the surface of the bare plate. Finally, the ultrasonically cleaned hot-formed steel bare plate is rinsed with running water and dried with a hair dryer to obtain the pre-treated bare plate;

[0067] (2) After confirming that the magnetron sputtering equipment is operating normally, place the pretreated bare plate in a specially sized magnetron sputtering target with a target-substrate distance of 150 mm. Then, perform vacuum treatment to a vacuum level better than 5 × 10⁻⁶. -4 Pa; Introduce 99.995% pure argon gas at a flow rate of 70 sccm, fix the substrate in the fixture, adjust the gate valve to bring the vacuum to about 0.3 Pa, set the rotation speed of the rotating frame to 5 r / min, turn on the ion source with a voltage of 750 V and a current of 0.25 A, and set the cleaning time to 30 min. End the cleaning process, turn off the ion source, and obtain a clean bare plate.

[0068] (3) Maintaining a constant rotation speed, adjust the gate valve to bring the vacuum level to approximately 0.8 Pa, turn on the bias voltage and set it to -100 V. Using Ti3Al alloy as the target material, apply direct current. The DC power supply sputtering power is 650 W, voltage is 380 V, current is 1.7 A, and sputtering time is 90 min. After the sputtering time is completed, wait for the temperature to cool to room temperature, then turn off the gate valve, molecular pump, and mechanical pump. Remove the sample to obtain a Ti3Al alloy coating sample with a coating thickness of 2 μm.

[0069] Example 2

[0070] This embodiment provides a method for preparing Ti3Al alloy-coated steel plates using magnetron sputtering, comprising the following steps:

[0071] (1) The hot-formed steel bare plate (the size of the hot-formed steel bare plate is 100mm×70mm×1.4mm) is simply sanded with sandpaper of grits 200#, 1000# and 3000#. After sanding with sandpaper of different grits, the oxides on the surface of the bare plate can be removed. Then, the bare plate is placed in acetone solution and cleaned with an ultrasonic cleaner for 30 minutes to remove dust and oil stains from the surface of the bare plate. Finally, the ultrasonically cleaned hot-formed steel bare plate is rinsed with running water and dried with a hair dryer to obtain the pre-treated bare plate;

[0072] (2) After confirming that the magnetron sputtering equipment is operating normally, place the pretreated bare plate in a specially sized magnetron sputtering target with a target-substrate distance of 130 mm. Then, perform vacuum treatment to a vacuum level better than 5 × 10⁻⁶ mm. -4 Pa; Introduce 99.995% pure argon gas at a flow rate of 70 sccm, fix the substrate in the fixture, adjust the gate valve to bring the vacuum to about 0.3 Pa, set the rotation speed of the rotating frame to 5 r / min, turn on the ion source with a voltage of 750 V and a current of 0.25 A, and set the cleaning time to 30 min. End the cleaning process, turn off the ion source, and obtain a clean bare plate.

[0073] (3) Maintaining a constant rotation speed, adjust the gate valve to bring the vacuum level to approximately 0.8 Pa, turn on the bias voltage and set it to -100 V. Using Ti3Al alloy as the target material, apply direct current. The DC power supply sputtering power is 650 W, voltage is 380 V, current is 1.7 A, and sputtering time is 90 min. After the sputtering time is completed, wait for the temperature to cool to room temperature, then turn off the gate valve, molecular pump, and mechanical pump. Remove the sample to obtain a Ti3Al alloy coating sample with a coating thickness of 2 μm.

[0074] Example 3

[0075] This embodiment provides a method for preparing Ti3Al alloy-coated steel plates using magnetron sputtering, comprising the following steps:

[0076] (1) The hot-formed steel bare plate (the size of the hot-formed steel bare plate is 100mm×70mm×1.4mm) is simply sanded with sandpaper of grits 200#, 1000# and 3000#. After sanding with sandpaper of different grits, the oxides on the surface of the bare plate can be removed. Then, the bare plate is placed in acetone solution and cleaned with an ultrasonic cleaner for 30 minutes to remove dust and oil stains from the surface of the bare plate. Finally, the ultrasonically cleaned hot-formed steel bare plate is rinsed with running water and dried with a hair dryer to obtain the pre-treated bare plate;

[0077] (2) After confirming that the magnetron sputtering equipment is operating normally, place the pretreated bare plate in a specially sized magnetron sputtering target with a target-substrate distance of 150 mm. Then, perform vacuum treatment to a vacuum level better than 5 × 10⁻⁶. -4 Pa; Introduce 99.995% pure argon gas at a flow rate of 70 sccm, fix the substrate in the fixture, adjust the gate valve to bring the vacuum to about 0.3 Pa, set the rotation speed of the rotating frame to 5 r / min, turn on the ion source with a voltage of 750 V and a current of 0.25 A, and set the cleaning time to 30 min. End the cleaning process, turn off the ion source, and obtain a clean bare plate.

[0078] (3) Maintaining a constant rotation speed, adjust the gate valve to bring the vacuum level to approximately 0.8 Pa, turn on the bias voltage and set it to -100 V. Using Ti3Al alloy as the target material, apply direct current. The DC power supply sputtering power is 700 W, voltage is 390 V, current is 1.8 A, and sputtering time is 80 min. After the sputtering time is completed, wait for the temperature to cool to room temperature, then turn off the gate valve, molecular pump, and mechanical pump. Remove the sample to obtain a Ti3Al alloy coating sample with a coating thickness of 2 μm.

[0079] Comparative Example 1

[0080] This comparative example provides a pretreated bare plate, which is the same as the pretreated bare plate prepared in step (1) of Example 1.

[0081] Comparative Example 2

[0082] This comparative example provides an aluminum-silicon coated steel sheet. The steel substrate of the aluminum-silicon coated steel sheet is the same as the pretreated bare plate prepared in step (1) of Example 1, and the thickness of the aluminum-silicon coating is about 10 μm.

[0083] Electrochemical corrosion tests were conducted on the samples obtained in Examples 1-3 and Comparative Examples 1-2, and the test data were compared and analyzed. The electrochemical corrosion tests used the potentiodynamic scanning method to determine the stable polarization curves of the corroded samples after immersion in a 3.5% (wt. / %) NaCl solution for 30 min. The scanning rate was 1 mV / s, and the working area of ​​the sample was 0.5 cm². 2 The experiment used a three-electrode system. The results of the electrochemical corrosion test are shown in Table 1.

[0084] Table 1 Results of electrochemical corrosion test on samples

[0085] Group Self-corrosion potential (Ecorr) / V <![CDATA[Corrosion current (Icorr) / (A / cm 2 )]]> Example 1 -0.572 <![CDATA[4.780×10 -7 ]]> Example 2 -0.591 <![CDATA[3.097×10 -7 ]]> Example 3 -0.561 <![CDATA[2.667×10 -7 ]]> Comparative Example 1 -0.779 <![CDATA[1.699×10 -5 ]]> Comparative Example 2 -0.778 <![CDATA[6.963×10 -7 ]]>

[0086] Figure 3 The polarization curves of the electrochemical corrosion test provided in Example 1 and Comparative Examples 1 and 2 of this application.

[0087] Depend on Figure 3 As shown in Table 1, the corrosion current of the pretreated bare plate sample in Comparative Example 1 is 2.9366 × 10⁻⁶. -5 A / cm 2 The corrosion current density of the aluminum-silicon coated sample in Comparative Example 2 was 6.963 × 10⁻⁶. -7 A / cm 2 The corrosion current density of the sample with a Ti3Al alloy coating deposited by magnetron sputtering in Example 1 was 4.780 × 10⁻⁶. -7 A / cm 2Meanwhile, the self-corrosion potential shifted significantly, and the corrosion current density decreased by two orders of magnitude and the same order of magnitude, respectively, compared to the bare plate and the aluminum-silicon coated sample. The experimental results indicate that the corrosion resistance of hot-formed steel is significantly improved due to the excellent corrosion resistance of titanium alloy itself in the magnetron sputtered Ti3Al alloy coated sample.

[0088] Furthermore, one or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:

[0089] In this embodiment of the invention, magnetron sputtering of Ti3Al alloy coating on the surface of hot-formed steel is a novel, efficient, and green anti-corrosion method that can effectively improve the corrosion resistance of hot-formed steel.

[0090] In this embodiment of the invention, the magnetron sputtering method for anti-corrosion of Ti3Al alloy coating can effectively improve the problems of easy oxidation, easy corrosion, and service life of traditional bare plates; improve the problems of zinc ash, zinc slag, zinc resource waste, and unstable surface quality of zinc-based coating products; and improve the problems of high production cost and poor processing plasticity of aluminum-silicon coatings. It can effectively improve the corrosion resistance of hot-formed steel, thereby significantly extending the service life of hot-formed steel products.

[0091] The above description is merely a specific embodiment of this application, enabling those skilled in the art to understand or implement this application. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of this application. Therefore, this application is not to be limited to the embodiments shown herein, but is to be accorded the widest scope consistent with the principles and novel features claimed herein.

Claims

1. A method for preparing Ti3Al alloy-coated steel sheets using magnetron sputtering, characterized in that, The method includes: The hot-formed steel bare sheet is pretreated to obtain a pretreated bare sheet. The pretreatment includes: grinding the hot-formed steel bare sheet step by step with sandpaper of grits of 200#, 1000# and 3000#, followed by ultrasonic cleaning and drying to obtain the pretreated bare sheet; the ultrasonic cleaning time is 25min~35min. Using Ti3Al alloy as the target material, the pretreated bare plate is subjected to magnetron sputtering to form a Ti3Al alloy-containing coating on at least a portion of the surface of the pretreated bare plate, thereby obtaining a Ti3Al alloy-coated steel plate. The process of using Ti3Al alloy as a target material to perform magnetron sputtering on the pretreated bare plate includes: The pretreated bare plate is placed in a vacuum chamber, and a magnetron sputtering Ti3Al alloy target is provided in the vacuum chamber. The distance between the pretreated bare plate and the magnetron sputtering Ti3Al alloy target is 120mm to 160mm. The pretreated bare plate was treated with the magnetron sputtering Ti3Al alloy target; The step of treating the pretreated bare plate with the magnetron sputtering Ti3Al alloy target includes: Adjust the vacuum level of the vacuum chamber to a first set vacuum level, wherein the first set vacuum level is < 5 × 10⁻⁶. -4 Pa; Argon gas is introduced into the vacuum chamber with a first set vacuum degree. The flow rate of the argon gas is 60 sccm to 80 sccm, and the vacuum degree is adjusted to a second vacuum degree. Then, the pre-treated bare plate is cleaned with a gas ion source to obtain a clean bare plate. The second vacuum degree is 0.25 Pa to 0.35 Pa. The parameters of the gas ion source cleaning are: rotation speed of the rotating frame 3 r / min to 6 r / min, voltage 720 V to 780 V, current 0.2 A to 0.4 A, and cleaning time 25 min to 35 min. Adjust the vacuum level of the vacuum chamber to the third set vacuum level, and adjust the bias voltage of the clean bare plate to the set bias voltage. The third set vacuum level is 0.75 Pa to 0.85 Pa, and the set bias voltage is -80 V to -120 V. Ti3Al alloy was magnetron sputtered and deposited on the clean bare plate using a DC power supply. The magnetron sputtering power was 600W to 750W and the sputtering time was 70min to 100min. The corrosion current density of the Ti3Al alloy-coated steel plate is ≤6.5×10⁻⁶. -7 A / cm 2 .

2. A Ti3Al alloy-coated steel sheet prepared by the method of claim 1, characterized in that, The Ti3Al alloy coated steel sheet includes a hot-formed steel bare sheet and a Ti3Al alloy coating covering at least a portion of the surface of the hot-formed steel bare sheet, wherein the thickness of the Ti3Al alloy coating is 1μm to 3μm.