High-mechanical porous structure electrolyte, preparation method and application thereof
By adding pore-forming agents and additives to the resin matrix to regulate the pore structure, a high-mechanical-strength porous electrolyte was prepared, which solved the problem of poor performance caused by the single pore structure in the existing technology. It achieved a balance between high mechanical properties and high ionic conductivity, and improved the performance of structural energy storage composite materials.
Patent Information
- Application Number
- CN202410746354.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2024-05-24
- Filing Date
- 2024-06-11
- Publication Date
- 2026-11-20
- Estimated Expiration
- 2044-06-11
AI Technical Summary
The existing structural electrolytes have a simple pore structure, which leads to a mutual constraint between mechanical properties and ionic conductivity, and cannot meet the performance requirements of structural energy storage composite materials.
By adding pore-forming agents and additives to the resin matrix, the pore structure is controlled, and a high-mechanical-strength porous electrolyte is prepared. Combined with an ionic liquid electrolyte, the ionic conductivity is improved.
A balance between high mechanical properties and high ionic conductivity was achieved, improving the electromechanical properties of structural energy storage composite materials.
Smart Images

Figure FT_1 
Figure FT_2
Abstract
Description
Technical Field
[0001] This invention belongs to the field of structural energy storage composite materials, specifically relating to a high-mechanical-strength porous electrolyte, its preparation method, and its application. Background Technology
[0002] Currently, aerospace vehicles and weaponry from various countries are facing higher demands for miniaturization, lightweighting, and intelligence. At present, equipment systems need to carry large and heavy battery packs to meet complex operational requirements, which to some extent restricts the reduction of equipment weight and the improvement of its intelligence level. On the other hand, for example, the aerospace field extensively uses carbon fiber composite materials to reduce fuselage weight. If these composite material structures can be utilized to provide energy output, a large portion of the battery pack weight can be eliminated, simultaneously meeting the requirements for lightweighting and intelligence.
[0003] Structural energy storage composite materials are a novel composite material system that integrates energy storage and load-bearing capacity, using a resin matrix as the structural electrolyte and carbon fiber as both reinforcement and electrode material. They possess the advantages of lithium-ion batteries, such as low cost, large theoretical energy storage capacity, rapid charge-discharge capability, and stable cyclic charge-discharge performance, while also exhibiting the lightweight and high strength of carbon fiber reinforced resin matrix composites. This effectively reduces system weight and saves system space, demonstrating enormous application potential and significant implications for achieving functionalization, lightweighting, and high performance in weaponry and aerospace vehicles. One of the key factors influencing the performance of structural energy storage composite materials is the structural electrolyte technology, which serves as both an ion transport channel and a means of transferring mechanical loads. An ideal structural electrolyte should possess both high mechanical strength and ionic conductivity.
[0004] Polymer-based gel electrolytes are currently a key research area. Extensive research has been conducted on copolymers of polyethylene oxide, polyvinyl alcohol, polyacrylonitrile, and electrolyte salts. However, these electrolytes cannot meet the process and performance requirements of structural energy storage materials. For example, Wan Jiayu et al. used a polyimide (PI) film with vertical channels as a matrix to construct a vertically channel-filled PEO-LiFTSI polymer electrolyte, achieving an ionic conductivity of 0.23 mS / cm. However, the electrolyte is self-supporting and cannot withstand high mechanical loads. Introducing a liquid conductive phase into a resin system with high strength and modulus can yield structural electrolytes with higher performance. This method involves pre-forming pores in the resin matrix and then filling them with a conductive liquid. Li Mengjie et al. prepared an epoxy resin-polyetheramine structural electrolyte with a Young's modulus of 0.52 GPa and an ionic conductivity of 0.57 mS / cm. Simultaneously, the addition of 10% wt LLTO nanoparticles increased the Young's modulus to 0.65 GPa and the ionic conductivity to 2.02 mS / cm.
[0005] Currently, the performance of structural electrolytes is not ideal, and the problem of mutual constraint between mechanical properties and ionic conductivity urgently needs to be solved. The fundamental factor is that ionic conductivity mainly depends on porosity, and increasing porosity directly leads to a reduction in resin matrix content. Based on the above problems, this invention proposes a method for regulating the pore structure of structural electrolytes to balance both performance parameters. Chinese patent application CN115763961A discloses a method for structural design by growing MOFs on the pore walls, in which a porous electrolyte is placed in a 2-methylimidazole solution containing Zn(CH3COO)2·2H2O and the MOF is grown in situ at 60°C. In this method, the MOF does not play a role in regulating the pore structure, and only proposes a method to control the pore size by changing the curing agent content. Summary of the Invention
[0006] To address the problem of poor electromechanical performance caused by the simple and unreasonable pore structure of existing electrolytes, this invention provides a high-mechanical-performance porous electrolyte, its preparation method, and its application.
[0007] A method for preparing a high-mechanical-strength porous electrolyte, the process of which is as follows: (1) Mix the resin with the pore-forming agent and additives and stir to form a uniform precursor solution; wherein the mass ratio of resin, pore-forming agent and additives is 1:(2~4):(0.01~0.1). (2) Mix the precursor solution with the curing agent and stir until homogeneous. The mass ratio of resin to curing agent is 1:(0.2~0.6). (3) The solution in step (2) is defoamed to obtain the precursor electrolyte; (4) The degassed precursor electrolyte is poured into a mold coated with a release agent, and a cover plate coated with the same release agent is placed on top of the mold to seal it. (5) The resin in the mold is cured, demolded, soaked in water to remove the pore-forming agent, and dehydrated to obtain porous resin; (6) After polishing the surface of the porous resin, immerse it in an ion electrolyte for more than 10 hours, then take it out to obtain the product.
[0008] Further, in step (1), the resin is one or a mixture of two or more of the following in any proportion: bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane resin, ethoxylated bisphenol A dimethacrylate, and 1,4-butanediol diacrylate.
[0009] Further, in step (1), the pore-forming agent is one or a mixture of two or more of polyethylene glycol 200 (PEG200), polyethylene glycol 150 (PEG150), diethylene glycol, and triethylene glycol in any proportion.
[0010] Further, in step (1), the additive is one or a mixture of two or more of 1,4-dioxane, N,N-dimethylamide, cyclohexanone, dimethyl sulfoxide, and diethyltoluenediamine in any proportion.
[0011] Further, in step (2), the curing agent is one or a mixture of two or more of 4,4'-diaminodicyclohexylmethane (PACM), 4,4'-diaminodiphenylmethane, azobisisobutyronitrile, and 2,2-dimethylolpropionic acid in any proportion.
[0012] When the resin is bisphenol A type epoxy resin, curing refers to curing at 110℃~190℃ for 2~4 hours; when the resin is bisphenol F type epoxy resin, curing refers to curing at 110℃~190℃ for 2~4 hours; when the resin is 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane resin, curing refers to curing at 130℃~180℃ for 2~4 hours.
[0013] The lithium hexafluorophosphate ion liquid electrolyte specifically refers to 1M LiPF6 in DEC:DMC:EC=1:1:1 Vol% with 1%VC, and the aluminum ion liquid electrolyte refers to imidazole chloroaluminate ion liquid, specifically 1-ethyl-3-methylimidazolium chloroaluminate ([EMIm]Cl / AlCl3 molar ratio 1:1.3).
[0014] The high-mechanical-strength porous electrolyte prepared by the above method.
[0015] The application of the aforementioned high-mechanical-strength porous electrolyte in structural energy storage composite materials.
[0016] The assembly process of the structural energy storage composite material is as follows: (1) The prepared carbon fiber positive electrode material is laid up according to the positive electrode material / glass fiber membrane / negative electrode material and then the precursor electrolyte is injected through the vacuum-assisted resin injection molding process to cure the resin. (2) Demold the cured resin, soak it in deionized water for 20-30 hours to remove the pore-forming agent, and then dry it; (3) The dried sample is immersed in lithium hexafluorophosphate ion liquid electrolyte or imidazole chloroaluminate ion liquid for 20h~30h to obtain carbon fiber lithium structure or aluminum structure energy storage composite material, and then aluminum plastic film is used to encapsulate the structure energy storage composite material.
[0017] Furthermore, the carbon fiber cathode is prepared by uniformly mixing (1~2) wt% carboxymethyl cellulose solution, natural graphite, conductive carbon black, and SBR binder at a mass ratio of 250:9:5:5, and then coating the mixture onto carbon fiber fabric, with a natural graphite loading of 10~15 mg / cm³.2 The diaphragm is Whatman glass fiber filter paper, and the negative electrode is a lithium sheet or aluminum metal mesh.
[0018] Furthermore, the coating amount of the precursor electrolyte is 50~100 mg / cm³. 2 The lithium hexafluorophosphate ion liquid electrolyte specifically refers to 1M LiPF6 in DEC:DMC:EC=1:1:1 Vol% with 1% VC. The aluminum ion liquid electrolyte refers to imidazole chloroaluminate ion liquid, specifically 1-ethyl-3-methylimidazolium chloroaluminate ([EMIm]Cl / AlCl3 molar ratio 1:1.3). Based on the mass of the resin electrolyte, the adsorption capacity of the liquid electrolyte is (0.5~2) g / g.
[0019] Compared with the prior art, the present invention has the following beneficial effects: This invention increases the compatibility of the system by adding a benign solvent to the resin, thereby increasing the cohesive energy between polymer molecules and delaying the phase separation process. As the solubility parameters and content of the additives increase, the pore size can be reduced, shifting from micron-sized mesopores to nano-sized micropores. Simultaneously, this invention also achieves porosity regulation by adding amine-based curing additives to control the curing rate. The porous resin electrolyte of this invention, when applied to structural energy storage composite materials such as structured batteries and supercapacitors, can effectively improve the electromechanical performance of structural energy storage devices. Attached Figure Description
[0020] Figure 1 In the middle: (a) is the tensile stress-strain curve of the structural electrolyte prepared in Example 1 of the present invention; (b) is the AC impedance spectrum of the structural electrolyte prepared in Example 1 of the present invention; Figure 2 The voltage-capacity diagram of the aluminum ion structure electrolyte prepared using the electrolyte obtained in Example 1 of this invention shows that the specific capacity of the first cycle is 61 mAh / g. Detailed Implementation
[0021] To enable those skilled in the art to better understand the technical solutions of the present invention, the preferred embodiments of the present invention are described below in conjunction with specific examples, but these should not be construed as limiting the present invention.
[0022] Example 1 A method for preparing a high-mechanical-strength porous electrolyte, the process of which is as follows: (1) Add 1 part of DGEBA epoxy resin (brand name: epoxy resin 0164) and 3 parts of polyethylene glycol 200 to a beaker and stir at room temperature for 25 minutes to obtain a completely homogeneous solution. Then add 0.33 parts of curing agent PACM and 0.07 parts of diethyltoluene diamine additive and mix and stir evenly. The content of each substance is based on the mass of resin.
[0023] (2) Place the mixed solution in a metal container and remove air bubbles using a vacuum pump for 5 minutes. To obtain rod-shaped specimens, pour the well-mixed solution into a metal mold, the mold shape of which should conform to ASTM D638 standard for tensile testing of plastics. Use a clean cover plate to slowly cover the mold surface from the side and clamp it tightly to seal. At the same time, to obtain film specimens, use a clean glass plate, with 0.42 mm thick gaskets bonded around its perimeter. After pouring the solution, cover and seal it with another glass plate.
[0024] (3) Place the sealed mold in an oven and cure at 160°C for 4 hours; after curing, cool it to room temperature in the oven.
[0025] (4) Remove the cured sample from the mold and soak it in distilled water to remove the water-soluble pore-forming agent. This process should last for at least 12 hours. After the pore-forming agent in the sample has been completely replaced, transfer it to a freeze dryer for dehydration treatment for 24 hours.
[0026] (5) Cut the porous resin in (4) into circular pieces with a diameter of 14 mm. Transfer the circular porous resin pieces to a glove box with an argon atmosphere and a water content and oxygen content of less than 0.01 ppm. Soak them in commercially available lithium-ion electrolyte for more than 12 hours. The formula is 1M LiPF6 in DEC:DMC:EC=1:1:1 Vol% with 1% VC. The preparation of the structural electrolyte is completed. After complete absorption of liquid, the electrolyte volume increases slightly.
[0027] (6) The electrochemical impedance spectroscopy of the disc samples was measured using an electrochemical workstation, and the ionic conductivity was calculated. Figure 1 (b) It can be seen that the ionic conductivity of the sample is 2.26 mS / cm.
[0028] (7) Tensile tests were performed on the rod-shaped specimens using a universal testing machine. The specimen dimensions conformed to GB / T1040 and ASTM D638 standards for tensile testing of plastics. The tensile stress-strain curve of the specimen is shown below. Figure 1 As shown in (a), by Figure 1 (a) It can be seen that the Young's modulus of the sample is 1.11 GPa and the tensile strength is 22.24 MPa.
[0029] (8) The porosity and density of the sample were tested using the density method. The calculation method is P = 1 - (ρ / ρ0), where ρ is the sample density and ρ0 is the density of the raw material resin. Example 1: The density of the raw material resin (DGEBA epoxy resin) was 1.19 g / cm³. 3 The sample density is 0.57 g / cm³. 3 The porosity is 52.1%.
[0030] Example 2 A method for preparing a high-mechanical-strength porous electrolyte, the process of which is as follows: (1) Add 1 part of DGEBA epoxy resin (brand name: epoxy resin 0164) and 3 parts of polyethylene glycol 200 to a beaker and stir at room temperature for 25 minutes to obtain a completely homogeneous solution. Then add 0.33 parts of curing agent PACM and 0.07 parts of DMF additive, and mix and stir evenly. The contents of each substance are based on the mass of resin.
[0031] (2) Place the mixed solution in a metal container and remove air bubbles using a vacuum pump for 5 minutes. To obtain rod-shaped specimens, pour the well-mixed solution into a metal mold, the mold shape of which should conform to ASTM D638 standard for tensile testing of plastics. Use a clean cover plate to slowly cover the mold surface from the side and clamp it tightly to seal. At the same time, to obtain film specimens, use a clean glass plate, with 0.42 mm thick gaskets bonded around its perimeter. After pouring the solution, cover and seal it with another glass plate.
[0032] (3) Place the sealed mold in an oven and cure at 160°C for 4 hours; after curing, cool it to room temperature in the oven.
[0033] (4) Remove the cured sample from the mold and soak it in distilled water to remove the water-soluble pore-forming agent. This process should last for at least 12 hours. After the pore-forming agent in the sample has been completely replaced, transfer it to a freeze dryer for dehydration treatment for 24 hours.
[0034] (5) Cut the porous resin in (4) into circular pieces with a diameter of 14 mm. Transfer the circular porous resin pieces to a glove box with an argon atmosphere and a water content and oxygen content of less than 0.01 ppm. Soak them in commercially available lithium-ion electrolyte for more than 12 hours. The formula is 1M LiPF6 in DEC:DMC:EC=1:1:1 Vol% with 1%VC. The preparation of the structural electrolyte is completed. After complete absorption of liquid, the electrolyte volume increases slightly.
[0035] (7) The electrochemical impedance spectroscopy of the disc sample was measured using an electrochemical workstation, and the ionic conductivity was calculated. The ionic conductivity of the sample was 1.83 mS / cm.
[0036] (8) Tensile tests were performed on the rod-shaped specimens using a universal testing machine. The specimen dimensions were in accordance with GB / T1040 and ASTM D638 standards for tensile testing of plastics. The Young's modulus of the specimens was 0.63 GPa.
[0037] (9) The porosity and density of the sample were tested using the density method. The calculation method is P = 1 - (ρ / ρ0), where ρ is the sample density and ρ0 is the density of the raw material resin without pore-forming agent. Example 2: The density of the raw material resin was 1.19 g / cm³. 3The sample density is 0.58 g / cm³. 3 The porosity is 51.3%.
[0038] An aluminum ion-structured energy storage composite material was assembled using the electrolyte structure obtained in Example 1. The preparation method is as follows: (1) The electrode materials are stacked in the manner of positive electrode-separator-negative electrode. The positive electrode material is T800 carbon fiber fabric coated with natural graphite (from Guangwei), with a size of 40mm*40mm. The L-shaped molybdenum current collector is bonded to the non-active material surface using conductive silver paste. The separator is Whatman glass fiber filter paper with a size of 60mm*60mm. The negative electrode is an aluminum metal mesh with a pore size of 0.3mm*0.6mm and a size of 45mm*45mm, and the current collector is led out.
[0039] The positive electrode is prepared as follows: ① First, a 1wt% solution of carboxymethyl cellulose is prepared by dissolving it in deionized water and stirring for 8 hours until completely dissolved. ② Natural graphite, SP conductive carbon black, and SBR binder are weighed and added to the carboxymethyl cellulose solution, then stirred for 48 hours to form a uniform slurry. ③ The slurry is uniformly coated onto carbon fiber fabric using an automatic coating machine to a thickness of 300 μm. It is then dried in a 60℃ forced-air oven for 24 hours to remove the solvent, yielding a carbon fiber positive electrode with a final loading of 12 mg / cm³. 2 .
[0040] (2) Electrolyte precursors were injected using the vacuum injection method. The injection amount for a single cell was approximately 0.9g. Curing was carried out in a forced-air oven according to the curing process corresponding to each electrolyte. After curing, the cells were cooled to room temperature in the oven.
[0041] (3) Soak the cured battery in distilled water for at least 24 hours, washing it several times during the process. Then dry it in a 60°C forced-air oven for 24 hours.
[0042] (4) The batteries were immersed in an ionic liquid in an argon atmosphere glove box for 24 hours. The ionic liquid was anhydrous aluminum chloride-1-ethyl-3-methylimidazolium chloride ionic liquid electrolyte (AlCl3:[EMIm]Cl=1.3:1 molar ratio, Duoduo Chemical reagent). After complete immersion, the batteries were sealed in an aluminum-plastic film inside the glove box to form a sealed structure. The immersion volume of a single battery was approximately 0.9g.
[0043] (5) Perform charge and discharge tests on the battery with a cycle rate of 0.02C and a cycle period of 50 times. Figure 2 The figure shows the voltage-capacity diagram of the aluminum ion structure electrolyte prepared using the electrolyte obtained in Example 1 of this invention. The specific capacity of the first cycle is 61 mAh / g, and the specific capacity after 50 cycles is 58 mAh / g, with a capacity retention rate of 95.1% and a coulombic efficiency of 98.5%.
[0044] The above description is only a partial embodiment of the present invention. For those skilled in the art, several improvements and substitutions can be made without departing from the principle of the present invention, and these improvements and substitutions should also be considered within the scope of protection of the present invention.
Claims
1. A method for preparing a high-mechanical-strength porous electrolyte, characterized in that, The process is as follows: (1) Mix epoxy resin DGEBA with pore-forming agent PEG200 and stir until uniform; then add curing agent 4,4'-diaminodicyclohexylmethane PACM and additive diethyltoluene diamine and stir until uniform; wherein, the mass ratio of resin, pore-forming agent and additive is 1:3:0.07, and the mass ratio of resin to curing agent is 1:0.
33. (2) The solution in step (1) is defoamed to obtain the precursor electrolyte; (3) The degassed precursor electrolyte is poured into a mold coated with a release agent, and a cover plate coated with the same release agent is placed on top of the mold to seal it. (4) The resin in the mold is cured, demolded, soaked in water to remove the pore-forming agent, and dehydrated to obtain porous resin; (5) After polishing the surface of the porous resin, immerse it in the ion electrolyte for more than 10 hours and take it out to obtain the product. The ion electrolyte is an anhydrous aluminum chloride-1-ethyl-3-methylimidazolium chloride ion liquid electrolyte with a molar ratio of 1M LiPF6 in DEC:DMC:EC=1:1:1 Vol% with 1%VC or AlCl3:[EMIm]Cl of 1.3:
1. The adsorption capacity of the liquid electrolyte is (0.5~2) g / g based on the mass of the resin electrolyte.
2. The high-mechanical-strength porous electrolyte obtained by the preparation method according to claim 1.
3. The application of a high-mechanical-strength porous electrolyte in structural energy storage composite materials, characterized in that, The assembly process of structural energy storage composite materials is as follows: (1) The prepared carbon fiber positive electrode material is laid up according to the positive electrode material / glass fiber membrane / negative electrode material and then the precursor electrolyte is injected through the vacuum-assisted resin injection molding process to cure the resin. (2) Demold the cured resin, soak it in deionized water for 20-30 hours to remove the pore-forming agent, and then dry it; (3) The dried sample is immersed in lithium hexafluorophosphate ion liquid electrolyte or imidazole chloroaluminate ion liquid for 20-30 hours to obtain carbon fiber lithium structure or aluminum structure energy storage composite material, and then the structure energy storage composite material is encapsulated with aluminum-plastic film; the carbon fiber positive electrode is prepared by mixing (1-2) wt% carboxymethyl cellulose solution, natural graphite, conductive carbon black and SBR binder in a mass ratio of 250:9:5:5, and then coating it on carbon fiber fabric, with a natural graphite loading of 10-15 mg / cm³. 2 The diaphragm is Whatman glass fiber filter paper, and the negative electrode is a lithium sheet or aluminum mesh. The precursor electrolyte is obtained through the following process: epoxy resin DGEBA is mixed with pore-forming agent PEG200 and stirred until homogeneous; then curing agent 4,4'-diaminodicyclohexylmethane PACM and additive diethyltoluene diamine are added and stirred until homogeneous; wherein, the mass ratio of resin, pore-forming agent and additive is 1:3:0.07, and the mass ratio of resin to curing agent is 1:0.33; the solution is degassed to obtain the precursor electrolyte, and the coating amount of the precursor electrolyte is 50~100 mg / cm³. 2 .
4. The application according to claim 3, characterized in that, The ionic electrolyte is an anhydrous aluminum chloride-1-ethyl-3-methylimidazolium chloride ionic liquid electrolyte with a molar ratio of 1M LiPF6 in DEC:DMC:EC=1:1:1 Vol% with 1% VC or AlCl3:[EMIm]Cl of 1.3:
1. The adsorption capacity of the liquid electrolyte is (0.5~2) g / g based on the mass of the resin electrolyte.
Citation Information
Patent Citations
Epoxy resin-based gel electrolyte as well as preparation method and application thereof
CN115763961A
Carbon fiber-aluminum structure energy storage integrated composite material and preparation method thereof
CN118039879A
Reinforcement type solid polymer electrolyte membrane and its manufacturing method