Antistatic film

By laminating an antistatic layer containing conductive polymers, crosslinking agents, and surfactants onto a polyester film, the problems of haze increase and electrostatic peeling in the processing of optical components are solved, and a protective film with high transparency and antistatic properties is achieved.

CN118647509BActive Publication Date: 2026-11-24TOYOBO CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202380020360.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-02-09
Filing Date
2023-01-20
Publication Date
2026-11-24
Estimated Expiration
2043-01-20

AI Technical Summary

Technical Problem

In the processing of optical components, existing antistatic films experience increased haze after the heating and drying process, resulting in reduced visibility, difficulty in visual inspection, and persistent problems with electrostatic peeling and foreign matter adhesion.

Method used

An antistatic layer is laminated on a polyester film. The antistatic layer contains a conductive polymer, a crosslinking agent, and a surfactant. The crosslinking agent is a melamine-based crosslinking agent, and the surfactant is an acetylene-based surfactant with an HLB value of less than 9, high crosslinking density, and inhibition of oligomer precipitation. The surface resistivity is 2 to 7 [logΩ/□].

Benefits of technology

It effectively suppresses the increase in haze after heating and drying, maintains high transparency, allows for visual inspection, prevents electrostatic peeling and foreign matter adhesion, and ensures the visibility and adhesion of the protective film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004978745430000081
    Figure BDA0004978745430000081
  • Figure BDA0004978745430000171
    Figure BDA0004978745430000171
  • Figure BDA0004978745430000181
    Figure BDA0004978745430000181
Patent Text Reader

Abstract

[Problem] To provide: an antistatic film and a protective film that suppresses haze increase even when the antistatic layer is thin, and has low surface resistivity after a heat drying process. [Solution] In one aspect of the present invention, a laminated polyester film having an antistatic layer on at least one side of a substrate is provided. The laminated polyester film is characterized in that the antistatic layer comprises at least a conductive polymer, a crosslinking agent, and a surfactant, wherein the surfactant has an HLB value of 9 or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to antistatic films and protective films having an adhesive layer laminated on the antistatic film, and particularly to protective films for optical components (e.g., organic EL, components of liquid crystal displays). Background Technology

[0002] Films formed by laminating adhesive layers onto a substrate film are used as protective films for various components during the manufacturing process of optical components, etc. The protective film adheres to the components, which are the adhered objects, via the adhesive layer, and plays a role in inhibiting scratches and dirt adhesion during the processing and transportation of the components. As the substrate film used in these protective films, an antistatic film with an antistatic layer laminated on at least one side is used. The purpose of laminating the antistatic layer is to prevent foreign matter such as debris and dust from adhering to the protective film and to suppress static electricity generated when the protective film is peeled off from the adhered object (see Patent Document 1).

[0003] As an antistatic film, an antistatic film containing PEDOT:PSS as an antistatic agent has been proposed (see Patent Document 2).

[0004] Existing technical documents

[0005] Patent documents

[0006] Patent Document 1: International Publication 2018 / 012545

[0007] Patent Document 2: Japanese Patent Application Publication No. 2018-172473 Summary of the Invention

[0008] The problem the invention aims to solve

[0009] Protective films with antistatic layers can be used as protective films for optical components, especially in the processing of components for displays. In recent years, they have also been increasingly used in the processing of components for organic EL displays (particularly OLED displays). To adhere the protective film to the optical component, an adhesive layer is provided on at least one side of the protective film, and the process of laminating the adhesive layer includes a heat drying process.

[0010] For example, when an adhesive layer is laminated on a protective film, oligomers may precipitate due to the heating and drying process, leading to increased haze and sometimes a deterioration in the film's appearance. As the haze of the protective film increases, visibility decreases, making visual inspection of the protective film adhered to the substrate difficult, thus posing a challenge.

[0011] In this invention, in response to the aforementioned problem of protective films, an antistatic film and a protective film are provided that, even when the antistatic layer is thin, suppress the increase of haze after the heating and drying process, and have low surface resistivity.

[0012] Solution for solving the problem

[0013] That is, the present invention comprises the following components.

[0014] [1] A polyester film, characterized in that it is a laminated polyester film having an antistatic layer on at least one side of a substrate, wherein the antistatic layer comprises at least a conductive polymer, a crosslinking agent, and a surfactant, wherein the HLB value of the surfactant is 9 or less.

[0015] [2] In one method, the aforementioned crosslinking agent is a melamine-based crosslinking agent.

[0016] [3] In one method, the aforementioned melamine-based crosslinking agent is a fully ether-type methylated melamine resin.

[0017] [4] In one embodiment, the surface resistivity of the aforementioned antistatic layer is 2 to 7 [logΩ / □].

[0018] [5] In one embodiment, the aforementioned surfactant is an acetylene-based surfactant.

[0019] [6] In one embodiment, the aforementioned conductive polymer is PEDOT:PSS (poly(3,4-ethylenedioxythiophene):poly(4-styrenesulfonate)).

[0020] [7] In one embodiment, a protective film has an adhesive layer laminated on at least one side of a polyester film.

[0021] The effects of the invention

[0022] According to the present invention, an antistatic film having an antistatic layer with oligomer end-capping properties laminated on at least one side of a polyester film is provided, thereby providing a protective film that allows for visual inspection even when the protective film with an adhesive layer laminated on the antistatic film is bonded to the adhered object, and suppresses peel charge and foreign matter adhesion during peeling. Detailed Implementation

[0023] The laminated polyester film (sometimes also called antistatic film) of the present invention is a material in which an antistatic layer is laminated on at least one side of a polyester film. Alternatively, an adhesive layer may be laminated on one side of the antistatic film, allowing it to be used as a protective film.

[0024] For example, when the laminated polyester film of the present invention is heated and dried in the adhesive layer lamination process, the haze of the protective film can be suppressed, so that visual inspection can be performed even when the protective film is attached to the object.

[0025] The present invention will now be described in detail.

[0026] (Polyester film)

[0027] The polyester film used as a substrate in this invention is a film mainly composed of polyester resin. Here, "film mainly composed of polyester resin" refers to a film formed from a resin composition containing 50% by mass or more of polyester resin; when blended with other polymers, it refers to a film containing 50% by mass or more of polyester resin; and when copolymerized with other monomers, it refers to a repeating constituent unit containing 50 mol% or more of polyester. Preferably, in the polyester film, the resin composition constituting the film contains 90% by mass or more, more preferably 95% by mass or more, and even more preferably 100% by mass of polyester resin.

[0028] As a polyester resin, the material is not particularly limited, and copolymers or blends formed by the condensation polymerization of dicarboxylic acid and diol components can be used. Examples of dicarboxylic acid components include terephthalic acid, isophthalic acid, phthalic acid, 2,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, diphenylcarboxylic acid, diphenoxyethanedicarboxylic acid, diphenylsulfonecarboxylic acid, anthracene dicarboxylic acid, 1,3-cyclopentanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, 1,4-cyclohexanedicarboxylic acid, hexahydroterephthalic acid, hexahydroisophthalic acid, malonic acid, dimethylmalonic acid, succinic acid, 3,3-diethylsuccinic acid, glutaric acid, 2,2-dimethylglutaric acid, adipic acid, 2-methyl adipic acid, trimethyl adipic acid, heptacyanic acid, azelaic acid, dimer acid, sebacic acid, octanoic acid, dodecanedicarboxylic acid, etc.

[0029] Examples of diols that constitute polyester resins include ethylene glycol, propylene glycol, hexamethylene glycol, neopentyl glycol, 1,2-cyclohexanediethanol, 1,4-cyclohexanediethanol, decamethyl glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 2,2-bis(4-hydroxyphenyl)propane, and bis(4-hydroxyphenyl)sulfone.

[0030] One or more dicarboxylic acid components and two glycol components can be used to constitute the polyester resin. In addition, other acid components such as trimellitic acid and other hydroxyl components such as trimethylolpropane can also be appropriately added.

[0031] Specifically, polyester resins include polyethylene terephthalate, polyethylene terephthalate, polyethylene terephthalate, polyethylene terephthalate, and polyethylene naphthalate. Among these, polyethylene terephthalate is preferred due to its balance between physical properties and cost.

[0032] To improve the handling properties of polyester films, such as slippage and winding, the films can contain inactive particles. However, for applications such as optical applications, it is preferable that the polyester film is substantially free of particles. When the polyester film is free of particles, it is preferable that the coating layer, formed by online coating, contains particles. By making the polyester film free of particles and the coating layer containing particles, transparency is improved, and visual inspection is easier, which is therefore preferred.

[0033] The haze of the polyester film used in this invention is preferably 3% or less. More preferably, it is 2.5% or less, and even more preferably, it is 2.0% or less. It is extremely preferred if it is 1.5% or less. If it is 3% or less, visual inspection can be performed while the protective film is bonded to the substrate, so it is preferred, especially when the substrate is a component for optical purposes.

[0034] The average surface roughness (Sa) of the polyester film used in this invention is preferably in the range of 1 to 40 nm, more preferably 1 to 30 nm, and even more preferably 1 to 10 nm. The maximum protrusion height (P) of the polyester film used in this invention is preferably 2 μm or less, more preferably 1.5 μm or less, and even more preferably 0.8 μm or less. When Sa is 40 nm or less and P is 2 μm or less, even when the adhesive layer is stacked and rolled into a roll, there is no need to worry about the adhesive surface becoming rough, which is preferred.

[0035] In this invention, the thickness of the polyester film is not particularly limited, but is preferably in the range of 12 to 188 μm. More preferably, it is 18 to 125 μm, and even more preferably, it is 25 to 100 μm. When it is 12 μm or more, there is no concern about introducing wrinkles when it is bonded to the substrate as a protective film, and when it is 188 μm or less, it is cost-effective.

[0036] The polyester film serving as the substrate can be a single layer or composed of two or more layers stacked together. Furthermore, various additives can be included in the film as needed, within the scope of achieving the effects of this invention. Examples of additives include antioxidants, lightfastness agents, anti-gelling agents, organic wetting agents, antistatic agents, ultraviolet absorbers, and surfactants. When the film has a laminated structure, it is also preferable to include additives as needed to address the function of each layer.

[0037] Polyester film can be obtained, for example, by melting and extruding the aforementioned polyester resin into a film shape, and then cooling and solidifying it on a casting drum to form a film. As the polyester film of the present invention, either unstretched film or stretched film can be used; however, stretched film is preferred from the perspective of durability, such as mechanical strength and chemical resistance. When the polyester film is a stretched film, the stretching method is not particularly limited, and methods such as longitudinal uniaxial stretching, transverse uniaxial stretching, sequential longitudinal and transverse biaxial stretching, and simultaneous longitudinal and transverse biaxial stretching can be used.

[0038] To improve adhesion to the bonding reinforcement layer, the surface of the polyester film can be treated with surface treatments such as anchor coating, corona treatment, plasma treatment, or flame treatment. When an anchor coating is used, online coating is preferred from a cost perspective.

[0039] (Antistatic layer)

[0040] The antistatic film of the present invention requires an antistatic layer to be laminated on at least one side of a polyester film. The antistatic layer may be laminated on only one side or on both sides. By laminating the antistatic layer, when the adhesive layer is laminated as a protective film, it is also possible to suppress peeling static electricity or foreign matter adhesion to the adhered object, which is therefore preferred.

[0041] An antistatic layer is a layer formed by curing at least a conductive polymer, a crosslinking agent, and a surfactant. Such compositions are sometimes referred to as compositions for forming antistatic layers.

[0042] There are no particular limitations on the method of layering antistatic layers. Known methods such as coating, vacuum evaporation, and lamination can be used. From a cost point of view, it is more preferable to use coating to set the coating liquid containing antistatic agent.

[0043] (Conductive polymer)

[0044] The conductive polymer in this invention is a polymer capable of imparting antistatic properties. It can be a cationic compound or other polymer utilizing ion conduction, or a π-electron conjugated system conductive polymer, etc., from the viewpoint of antistatic properties under low humidity. A π-electron conjugated system conductive polymer is preferred. Furthermore, π-electron conjugated system conductive polymers can maintain antistatic properties at a high level without depending on moisture in the air, thus exhibiting good antistatic properties in various operating environments of the protective film, and are therefore preferred.

[0045] Furthermore, antistatic agents may be used in combination without compromising the effectiveness of the conductive polymer of the present invention. As antistatic agents, they may be cationic compounds other than the conductive polymer of the present invention, polymers utilizing ion conduction, π-electron conjugated systems, and may include surfactants, silicon oxide compounds, conductive metal compounds, etc.

[0046] Examples of π-electron conjugated conductive polymers include aniline-based polymers containing aniline or its derivatives as constituent units, pyrrole-based polymers containing pyrrole or its derivatives as constituent units, acetylene-based polymers containing acetylene or its derivatives as constituent units, and thiophene-based polymers containing thiophene or its derivatives as constituent units. For high transparency, polymers without nitrogen atoms are preferred as π-electron conjugated conductive polymers. From a transparency perspective, thiophene-based polymers containing thiophene or its derivatives as constituent units are preferred, and polyalkylene dioxythiophene is particularly preferred. Examples of polyalkylene dioxythiophene include polyethylene dioxythiophene, polypropylene dioxythiophene, and poly(ethylene / propylene) dioxythiophene.

[0047] It should be noted that in thiophene-based polymers containing thiophene or its derivatives as constituent units, to improve antistatic properties, a dopant of 0.1 to 500 parts by mass can be blended relative to, for example, 100 parts by mass of the polymer containing thiophene or its derivatives as constituent units. Excessive amounts hinder electron movement, thus reducing antistatic properties; conversely, insufficient amounts reduce dispersibility in solvents. Examples of such dopants include LiCl and R... 1- 30 COOLi(R 1-30 : saturated hydrocarbon groups with 1 or more carbon atoms and less than 30 carbon atoms), R 1-30 SO3Li, R 1-30 COONa, R 1-30 SO3Na, R 1- 30 COOK, R 1-30 SO3K, tetraethylammonium, I2, BF3Na, BF4Na, HClO4, CF3SO3H, FeCl3, tetracyanoquinoline (TCNQ), Na2B 10 Cl 10 Phthalocyanine, porphyrin, glutamic acid, alkyl sulfonates, polystyrene sulfonate Na(K,Li) salt, styrene-styrene sulfonate Na(K,Li) salt copolymer, polystyrene sulfonate anion, styrene sulfonate-styrene sulfonate anion copolymer, etc.

[0048] In this invention, the conductive polymer contained in the antistatic layer preferably comprises 5% by mass or more, more preferably 10% by mass or more, relative to 100% by mass of all solid components in the antistatic layer. It should be noted that when using a π-electron conjugated system conductive polymer as the antistatic agent, and when using the aforementioned dopant, the content of the π-electron conjugated system conductive polymer in the antistatic layer specified in this application is the sum of the conductive polymer and the aforementioned dopant.

[0049] By including an antistatic agent in such a quantity, good antistatic properties can be imparted.

[0050] In this invention, the conductive polymer contained in the antistatic layer is preferably 50% by mass or less, more preferably 40% by mass or less, relative to 100% of the total solid components in the antistatic layer. It should be noted that when using a π-electron conjugated conductive polymer as the antistatic agent, and when using the aforementioned dopant, the content of the π-electron conjugated conductive polymer in the antistatic layer as specified in this application is the sum of the conductive polymer and the aforementioned dopant.

[0051] By including the antistatic agent in such an amount, it does not interact with the crosslinking agent, the coating liquid is less likely to aggregate, the antistatic layer has fewer defects, and high transparency can be maintained.

[0052] (Cross-linking agent)

[0053] In this invention, the antistatic layer is formed from a composition containing a crosslinking agent in order to form a crosslinked structure within it. The presence of a crosslinking agent improves durability and suppresses the decrease in antistatic performance even under high temperature and high humidity conditions, making it preferable. Specific crosslinking agents include urea-based, epoxy-based, melamine-based, isocyanate-based, oxazoline-based, carbodiimide-based, and aziridine-based agents. In one embodiment, a melamine-based crosslinking agent is preferred, and to increase the crosslinking density of the antistatic layer, it is preferable to increase the reactivity of the melamine-based crosslinking agent. Highly reactive melamine-based crosslinking agents will be described later. Furthermore, catalysts or the like can be appropriately used to promote the crosslinking reaction as needed.

[0054] As the melamine-based crosslinking agent used in the antistatic layer of this invention, any general melamine-based crosslinking agent can be used, without particular limitation. Preferably, it is a compound obtained by condensing melamine with formaldehyde, having one or more triazine rings and hydroxymethyl and / or alkoxymethyl groups per molecule. Specifically, it is preferable to form a compound by dehydrating and condensing a hydroxymethyl melamine derivative obtained by condensing melamine with formaldehyde with a lower alcohol such as methanol, ethanol, isopropanol, or butanol, and then etherifying it. Examples of hydroxymethylated melamine derivatives include monomethylol melamine, dimethylol melamine, trimethylol melamine, tetramethylol melamine, pentamethylol melamine, and hexamethylol melamine. One or more of these can be used.

[0055] To improve the reactivity of melamine-based crosslinking agents and increase the crosslinking density of the antistatic layer, hydroxymethyl methylated melamine or hexaalkoxymethyl melamine with more crosslinking sites per molecule is preferred, hexaalkoxymethyl melamine with superior reactivity is more preferred, and hexamethoxymethyl melamine is particularly preferred. Here, hexahydroxymethyl melamine refers to melamine in which X is hydroxymethyl (-CH2-OH) in formula (a) below. Hexaalkoxymethyl melamine refers to melamine formed by dehydration condensation reaction of an alcohol with a hydroxymethyl melamine derivative, where X is (-CH2-OR, R is an alkyl group having 1 to 4 carbon atoms). Hexamethoxymethyl melamine refers to melamine in which X is (-CH2-OMe).

[0056]

[0057] In (a) above, X can be the same or different. Additionally, R can be the same or different. Furthermore, X can also be (-H).

[0058] The melamine-based crosslinking agent used in this invention is not a single compound, but preferably a mixture of multiple compounds. Based on the structure of the main component of the melamine-based compound, it can be broadly classified into all-ether type (X = -CH2-OR, R is an alkyl group with 1 to 4 carbon atoms), hydroxymethyl type (X = -CH2-OH), imino type (X = -H), and imino·hydroxymethyl type.

[0059] In one approach, from a reactivity point of view, the use of a fully etherified or hydroxymethylated melamine is preferred, with the fully etherified type being more preferred. Among the fully etherified types, hexamethoxymethyl melamine (CAS No. 3089-11-0), in which R is methyl, is most preferred. The higher the content of hexamethoxymethyl melamine in the melamine-based compound used, the more reactive and densely crosslinked the antistatic layer can be formed.

[0060] In the antistatic layer of this invention, the melamine-based crosslinking agent preferably has a weight-average degree of polymerization of 2.5 or less, more preferably 2.3 or less, and even more preferably 2.0 or less. A weight-average degree of polymerization of 2.5 or less allows for good compatibility with conductive polymers, and also inhibits the aggregation of the coating solution, resulting in a film with fewer defects.

[0061] Furthermore, in this invention, if the weight-average degree of polymerization is below 2.5, the content of mononuclear bodies contained in the melamine-based crosslinking agent increases, thereby forming an antistatic layer with excellent reactivity, improved crosslinking density, and low oligomer precipitation, which is therefore preferred.

[0062] For example, the weight-average degree of polymerization can be above 1.1, and can exceed 1.5.

[0063] Melamine-based crosslinking agents sometimes contain imino groups (-NH2-) or polynuclear molecules during their synthesis. These melamine derivatives can be mixed, provided the weight-average degree of polymerization of the melamine-based crosslinking agent is within the aforementioned range. They also exhibit excellent reactivity and can be used individually.

[0064] In the antistatic layer of this invention, the melamine-based crosslinking agent preferably comprises 50% to 95% by mass, more preferably 55% to 95% by mass, and even more preferably 60% to 95% by mass, relative to 100% by mass of all solid components in the antistatic layer. By including 50% or more of the melamine-based crosslinking agent, the antistatic layer can achieve a high crosslinking density through the self-crosslinking of the melamine-based crosslinking agent, resulting in a dense antistatic layer. Therefore, oligomer precipitation can be suppressed, which is preferable. Here, "all solid components of the antistatic layer" refers to the total solid components of the melamine-based crosslinking agent and the conductive polymer, since a considerable portion of the solvent and surfactant will evaporate during the drying process.

[0065] In the antistatic layer of this invention, a composition containing a surfactant is formed to improve appearance. Examples of surfactants include silicone surfactants, fluorinated surfactants having perfluoroalkyl groups, hydrocarbon surfactants, and acetylene surfactants.

[0066] It is particularly desirable to include acetylene-based surfactants. By including acetylene-based surfactants, when this antistatic film is used as a protective film, migration to the protected product can be prevented, and adverse effects on the final product can be reduced.

[0067] The protective film on which the adhesive layer is laminated on the antistatic film of the present invention is used in the manufacturing process of optical components, etc. Therefore, as a surfactant used in the antistatic layer in a manner that does not contaminate the manufacturing process, an acetylene-based surfactant belonging to the hydrocarbon family is preferred. Examples of commercially available acetylene-based surfactants include the Sufynol series and the Olfine series (Nikshin Chemical Industry Co., Ltd.).

[0068] The surfactant contained in the antistatic layer of this invention has an HLB value of 9 or less. More preferably, it has an HLB value of 8 or less. By containing a surfactant with an HLB value of 9 or less, oligomers are less likely to precipitate onto the film surface, resulting in an antistatic film with low haze, which is therefore preferred. While this should not be theoretically explained, it is generally believed that the high polarity of the oligomers contained in the polyester film, coupled with a higher HLB value, leads to better compatibility between the surfactant and the oligomers. Consequently, when the surfactant is oriented on the coating surface, the oligomers also precipitate onto the coating surface, thus increasing the amount of oligomer precipitation. In this invention, the upper limit of the HLB value that can suppress the amount of oligomer precipitation was determined, and the invention was thus completed.

[0069] The surfactant contained in the antistatic layer of this invention preferably has an HLB value of 3 or higher, more preferably 4 or higher. If the HLB value is too low, its ability as a surfactant is reduced, resulting in poor appearance. By using a surfactant with an HLB value of 3 or higher, the dispersibility of the antistatic layer coating liquid will not deteriorate, which is preferable.

[0070] It should be noted that the HLB value (Hydrophile-Lipophile Balance) represents the balance between hydrophilicity and hydrophobicity, and is calculated using various methods such as the Griffith method and the Davis method.

[0071] Using surfactants with an HLB value of 9 or lower allows for a better balance between oligomer precipitation and coating appearance. PEDOT / PSS is preferred when used in conductive polymers. Furthermore, melamine is preferred as a crosslinking agent. This is believed to be due to the good balance between the compatibility of each material and the surfactant.

[0072] For example, by including a surfactant having the above-mentioned HLB and a melamine-based crosslinking agent, the antistatic layer in this invention can reduce the film thickness, further maintain the coating strength, and suppress the precipitation of oligomers contained in the polyester film.

[0073] In addition, the antistatic properties required for the antistatic layer can be well maintained before and after heating and after alcohol treatment.

[0074] In addition to the above, the antistatic layer may also contain lubricants, pigments, ultraviolet absorbers, silane coupling agents, etc., as needed, without hindering the purpose of the present invention.

[0075] The antistatic layer does not actually contain any organosilicon compounds.

[0076] In this invention, "substantially free of organosilicon compounds" is defined as having a content of less than 50 ppm when quantifying Si element using fluorescence X-ray analysis, preferably less than 10 ppm, and most preferably below the detection limit. This is because even without actively adding organosilicon components to the antistatic layer, there is a possibility that contaminants from foreign sources, dirt adhering to the production line or equipment in the manufacturing process of the raw resin or film can peel off and mix into the antistatic layer.

[0077] By making the antistatic layer substantially free of organosilicon compounds, the migration of organosilicon to the protected product can be prevented when the antistatic film is used as a protective film, thereby reducing the adverse effects on the final product.

[0078] The thickness of the antistatic layer of the present invention is preferably 0.005 μm or more and 1 μm or less. More preferably, it is 0.01 μm or more and 0.5 μm or less, and even more preferably, it is 0.01 μm or more and 0.2 μm or less. When the thickness of the antistatic layer is 0.005 μm or more, an antistatic effect can be obtained, which is preferred. On the other hand, when it is 1 μm or less, less coloring and higher transparency are achieved, which is also preferred.

[0079] Here, the laminated polyester film of the present invention is characterized in that the surfactant has an HLB value of 9 or less. By using a surfactant with an HLB value of 9 or less, it is possible to provide a protective film that, even when heated during the antistatic layer processing, does not easily precipitate oligomers on the film surface, and even when the antistatic layer is thin, exhibits minimal haze increase after heating. Furthermore, it allows for visual inspection even when the protective film with an adhesive layer laminated on it is bonded to the adhered object, and suppresses peel charge and foreign matter adhesion during peeling.

[0080] The haze of the laminated polyester film of the present invention is preferably 3.0% or less. More preferably 2.0% or less, and even more preferably 1.5% or less. It is extremely preferred if it is 1.0% or less. If it is 3.0% or less, visual inspection can be performed while the protective film is bonded to the substrate, so it is preferred, especially when the substrate is a component for optical applications. The haze can be 0, for example, it can be 0.1% or more.

[0081] The haze of the laminated polyester film of the present invention after heating at 140°C for 10 minutes is preferably 3.0% or less. More preferably, it is 2.5% or less, and even more preferably, it is 2.0% or less. It is extremely preferred if it is 1.5% or less. If it is 3.0% or less, visual inspection can be performed while the protective film is bonded to the substrate, so it is preferred, especially when the substrate is a component for optical applications. The haze after heating at 140°C for 10 minutes can be 0, for example, it can be 0.1% or more.

[0082] This should not be interpreted as a specific theory, but by incorporating the antistatic layer of this invention, an antistatic layer with excellent reactivity, improved crosslinking density, and reduced oligomer precipitation can be obtained. It is speculated that this can suppress the significant increase in haze after heating at 140°C for 10 minutes.

[0083] For example, the Δhaze value obtained by subtracting the haze of the laminated polyester film before heating from the haze after heating at 140°C for 10 minutes can be greater than -0.2 and less than 2.5, for example, greater than -0.2 and less than 1.6. By having the Δhaze value within such a range, an antistatic layer in which oligomers are less likely to precipitate can be obtained.

[0084] By forming an antistatic layer that prevents oligomers from precipitating, the following effects can be achieved: the visibility of the protective film is not easily reduced during the adhesive layer lamination process after heating and drying, and visual inspection can be performed even when the protective film is adhered to the object.

[0085] The surface resistivity of the antistatic layer of the present invention is 7 [logΩ / □] or less. More preferably, it is 6.5 [logΩ / □] or less, and even more preferably, it is 6 [logΩ / □] or less. By making the surface resistivity 7 [logΩ / □] or less, it is possible to suppress the charging of the protective film, prevent the adhesion of foreign matter during the process, and further suppress the adverse electrical effects of the charging of the protective film on the protected product.

[0086] Furthermore, the lower limit of the surface resistivity of the antistatic film is not particularly limited, but it is preferably 2 [logΩ / □] or higher. If the surface resistivity of the antistatic film is lower than 2 [logΩ / □], the processing cost of the antistatic layer will increase, so it is not preferred.

[0087] The total light transmittance of the antistatic film used in this invention is preferably 80% or more. More preferably, it is 85% or more, and even more preferably, it is 88% or more. When it is 80% or more, it is possible to perform visual inspections while the protective film is bonded to the object, and therefore it is preferred, especially when the object being bonded is a component for optical applications.

[0088] The change in surface resistivity of the antistatic layer after wiping with alcohol is preferably 1.3 times or less. More preferably 1.2 times or less, and even more preferably 1.1 times or less. When it is 1.3 times or less, even if alcohol is used in processes such as bonding, the initial surface resistivity is maintained when it becomes a protective film, which is therefore preferred.

[0089] The average surface roughness (Sa) of the surface of the antistatic layer is preferably in the range of 1 to 40 nm, more preferably 1 to 30 nm. Even more preferably 1 to 10 nm. The maximum protrusion height (P) of the surface of the antistatic film used in this invention is preferably 2 μm or less, more preferably 1.5 μm or less. Even more preferably 0.8 μm or less. When Sa is 40 nm or less and P is 2 μm or less, even when the adhesive layer is stacked and rolled into a roll, there is no need to worry about the adhesive surface becoming rough, which is preferable.

[0090] As a method for coating an antistatic layer onto the surface of a substrate film, there are methods such as gravure coating, reverse roller coating, air knife coating, dip coating, rod coating, and spin coating, in which a coating solution containing the aforementioned antistatic agent, binder resin, etc., is dispersed / dissolved in a solvent. The coating method suitable for conductive compositions is not particularly limited. Furthermore, the coating layer can be applied in an online coating process during film manufacturing or in an offline coating process after film manufacturing.

[0091] Regarding the antistatic layer, the drying temperature for forming the antistatic layer by the above method is typically 60°C or higher and 150°C or lower, preferably 90°C or higher and 140°C or lower. From the viewpoint of enabling processing in a short time and improving productivity, this temperature of 60°C or higher is preferred. Furthermore, when a crosslinking agent is included, the crosslinking reaction proceeds sufficiently, which is therefore preferable. On the other hand, when the temperature is below 150°C, the planarity of the film is maintained, which is also preferable.

[0092] An adhesive layer can be laminated by applying an adhesive to the laminated polyester film of the present invention and allowing it to cure. The adhesive can be used without particular limitation, and the resulting laminated film can be used as a protective film. The laminated adhesive layer can be any side of the antistatic film. When using an antistatic film with an antistatic layer on only one side, it is preferable to have the antistatic layer on the side of the antistatic film opposite to the side with the laminated adhesive layer.

[0093] Alternatively, ceramic sheets, resin films, etc., can be laminated on the antistatic layer of the laminated polyester film of the present invention.

[0094] Example

[0095] To illustrate the present invention in detail, the following embodiments are provided, but the present invention is not limited to these embodiments. It should be noted that the evaluation method used in the present invention is as follows.

[0096] (Surface resistivity)

[0097] Regarding the surface resistivity of the antistatic film surface of the present invention, after conditioning for 24 hours at 23°C and 55% humidity, the surface resistivity of the antistatic layer surface was measured using a simple low resistivity meter (Nittoseiko Analytech Co., Ltd., Loresta AX MCP-370), and evaluated according to the following criteria. If the surface resistivity exceeds 6 [logΩ / □], it is measured using a surface resistivity tester (SIMCO JAPAN, Worksurface Tester ST-3).

[0098] ◎: Surface resistivity is 2 or higher and 4 or lower [logΩ / □]

[0099] ○: Surface resistivity exceeding 4 and below 7 [logΩ / □]

[0100] △: Surface resistivity exceeds 7 [logΩ / □]

[0101] (Total transmittance, haze)

[0102] The total transmittance and haze of the film of the present invention were measured based on JIS K 7136 using a turbidimeter (Nippon Denshoku Corporation, NDH7000II) before and after heat treatment at 140°C for 10 minutes.

[0103] (Alcohol resistance)

[0104] The surface resistivity of the film of the present invention was measured before and after wiping it back and forth 10 times with ethanol-soaked wiping paper. Furthermore, the appearance change after the above treatment was evaluated according to the following criteria.

[0105] ◎: Almost no change

[0106] 〇: Slight changes

[0107] △: There is a change

[0108] ×: Changes in the degree of peeling and flaking of the antistatic layer.

[0109] (Example 1)

[0110] The antistatic coating liquid was obtained by mixing the amounts recorded in Table 2.

[0111] (Antistatic coating solution)

[0112] 18.31 parts by weight of water

[0113] 42.71 parts by weight of isopropanol

[0114] 33.3 parts by weight of conductive polymer

[0115] Crosslinking agent A-1 (manufactured by NIPPON CARBIDE INDUSTRIES CO.,INC., imino-methylated melamine resin, solid content concentration 80% by mass) 0.75 parts by mass

[0116] 4.5 parts by weight of conductive additive

[0117] Surfactant B-1 (manufactured by Nissin Chemical Industry Co., Ltd., acetylene-based, surface tension 26 mN / m, solid content concentration 100% by mass) 0.4 parts by mass

[0118] (Formation of the antistatic layer)

[0119] Using a gravure coating machine, the obtained antistatic coating liquid is coated on one side of A4360 (Cosmoshine (registered trademark), manufactured by Toyobo Co., Ltd.) with a thickness of 75μm, so that the wet film thickness is 9.0μm. It is then dried and cured in a hot air drying oven at 140°C for 30 seconds to obtain a polyester film with an antistatic layer.

[0120] (Example 2)

[0121] Surfactant B-2 (manufactured by Nissin Chemical Industry Co., Ltd., acetylene-based, surface tension 32 mN / m, solid content concentration 81%) was set according to the composition in Table 2. Except for this, an antistatic layer was formed by the same steps as in Example 1.

[0122] (Example 3)

[0123] Crosslinking agent A-2 (made by NIPPON CARBIDE INDUSTRIES CO.,INC., hydroxymethyl methylated melamine resin, solid content 70% by mass) was set according to the composition in Table 2. Otherwise, an antistatic layer was formed by the same steps as in Example 1.

[0124] (Example 4)

[0125] Crosslinking agent A-2 is set according to the composition in Table 2. Otherwise, an antistatic layer is formed by the same steps as in Example 2.

[0126] (Example 5)

[0127] Crosslinking agent A-3 (made by NIPPON CARBIDE INDUSTRIES CO.,INC., all-ether methylated melamine resin, solid content 70% by mass) was set according to the composition in Table 2. Otherwise, an antistatic layer was formed by the same steps as in Example 1.

[0128] (Example 6)

[0129] Crosslinking agent A-3 is set according to the composition in Table 2. Otherwise, an antistatic layer is formed by the same steps as in Example 2.

[0130] (Example 7)

[0131] Crosslinking agent A-4 (made by NIPPON CARBIDE INDUSTRIES CO.,INC., imino-hydroxymethyl methylated melamine resin, solid content 70% by mass) was set according to the composition in Table 2. Otherwise, an antistatic layer was formed by the same steps as in Example 1.

[0132] (Example 8)

[0133] Crosslinking agent A-4 is set according to the composition in Table 2. Otherwise, an antistatic layer is formed by the same steps as in Example 2.

[0134] (Examples 9 and 10)

[0135] According to the composition in Table 2, crosslinking agent A-3 was set as the binder resin, MD1200 (manufactured by Toyobo Co., Ltd., solid content 35% by mass) was set as the binder resin, and surfactant B-1 was set as the surfactant. Otherwise, an antistatic layer was formed by the same steps as in Example 1.

[0136] (Refer to Example 1)

[0137] Surfactant B-3 (manufactured by Nissin Chemical Industry Co., Ltd., acetylene-based, surface tension 28 mN / m, solid content concentration 75% by mass) was set according to the composition in Table 2. Except for this, an antistatic layer was formed by the same steps as in Example 1.

[0138] (See Example 2 for reference)

[0139] Crosslinking agent A-2 was set according to the composition in Table 2. Otherwise, an antistatic layer was formed by the same steps as in Comparative Example 1.

[0140] (Refer to Example 3)

[0141] Surfactant B-4 (made by Dow Toray Co., Ltd., silicone-based, surface tension 21 mN / m, solid content 100% by mass) was prepared according to the composition in Table 2. Otherwise, an antistatic layer was formed by the same steps as in Comparative Example 2.

[0142] (Refer to Example 4)

[0143] Crosslinking agent A-3 was set according to the composition in Table 2. Otherwise, an antistatic layer was formed by the same steps as in Comparative Example 1.

[0144] (Refer to Example 5)

[0145] Crosslinking agent A-3 was set according to the composition in Table 2. Otherwise, an antistatic layer was formed by the same steps as in Comparative Example 3.

[0146] (Refer to Example 6)

[0147] Crosslinking agent A-4 was set according to the composition in Table 2. Otherwise, an antistatic layer was formed by the same steps as in Comparative Example 1.

[0148] (Refer to Example 7)

[0149] Crosslinking agent A-4 was set according to the composition in Table 2. Otherwise, an antistatic layer was formed by the same steps as in Comparative Example 3.

[0150] [Table 1]

[0151] serial number HLB value B-1 8 B-2 6 B-3 10~13 B-4 11.5

[0152] [Table 2A]

[0153]

[0154] [Table 2B]

[0155]

[0156] [Table 3A]

[0157]

[0158] [Table 3B]

[0159]

[0160] It should be understood that the embodiments and examples disclosed herein are illustrative in all respects and are not restrictive. The scope of the invention is not shown by the above embodiments, but by the claims, and is intended to include all modifications of the same meaning and scope as the claims.

[0161] The laminated polyester film of the present invention obtained in the embodiments provides an antistatic film with an antistatic layer having low haze after heating laminated on at least one side of the polyester film, thereby enabling visual inspection, suppression of peel charge during peeling, and foreign matter adhesion when an adhesive layer is laminated on the antistatic film and used as a protective film.

[0162] It should be noted that the surfactants in Reference Examples 1 to 7 have HLB values ​​exceeding 9, and therefore tend to have higher haze after heating compared to the samples used in the examples.

[0163] Industrial availability

[0164] This invention relates to antistatic films and adhesive films having an adhesive layer laminated on the antistatic film, and particularly to protective films for optical components (e.g., organic EL, components of liquid crystal displays).

Claims

1. A laminated polyester film, characterized in that, It is a laminated polyester film having an antistatic layer on at least one side of a substrate. The antistatic layer comprises at least a conductive polymer, a crosslinking agent, and a surfactant. The crosslinking agent is a melamine-based crosslinking agent. In the antistatic layer, the melamine-based crosslinking agent comprises more than 50% and less than 95% by mass relative to 100% of the total solid components in the antistatic layer. The surfactant has an HLB value of 9 or less.

2. The laminated polyester film according to claim 1, wherein, The surface resistivity of the antistatic layer is 2~7 [logΩ / □].

3. The laminated polyester film according to claim 1, wherein, The surfactant is acetylene-based.

4. The laminated polyester film according to claim 1, wherein, The conductive polymer is PEDOT:PSS (poly(3,4-ethylenedioxythiophene):poly(4-styrenesulfonate)).

5. The laminated polyester film according to claim 1, wherein, The crosslinking agent is a fully ether-type methylated melamine resin.

6. A protective film having an adhesive layer laminated on at least one side of the polyester film according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Adhesive film for display protection

    JP2018172473A

  • Antistatic polyester film, and production method thereof

    JP2016186072A